Journal of Welding and Joining

Search

Close

Warning: fopen(/home/virtual/kwjs/journal/upload/ip_log/ip_log_2025-02.txt): failed to open stream: Permission denied in /home/virtual/lib/view_data.php on line 100 Warning: fwrite() expects parameter 1 to be resource, boolean given in /home/virtual/lib/view_data.php on line 101
Song and Nam: Machine Learning Algorithm Comparison for the Performance Evaluation of Manual Welding Process

Machine Learning Algorithm Comparison for the Performance Evaluation of Manual Welding Process

Chang Sub Song*, Jong-Ho Nam**,
Received September 20, 2023       Accepted December 11, 2023
ABSTRACT
With the development of technology, the shipbuilding industry has seen a rise in automated welding processes. However, manual welding continues to be a necessary and in-demand skill. Unfortunately, the supply of both high-skilled and unskilled welders has steadily declined over the past decade, leading to a shortage of professional manpower. To address the issue of manpower shortage, a proposal has been made to provide timely and efficient training program for unskilled welders. However, evaluating the effectiveness of the training has proven challenging due to the lack of clear criteria for assessing the performance. This paper conducts an effective performance evaluation of unskilled welders using powerful machine learning algorithms. The evaluation is based on a dataset collected from both high-skilled and unskilled welder groups in manual welding processes. A comparison study is conducted to determine the most suitable algorithm. The goal is to identify the positive and negative parameters in the training of the manual welding process and provide an effective education strategy for unskilled welders. Additionally, the paper aims to find the algorithm with the highest accuracy. Overall, this study seeks to provide a solution to the shortage of manual welding professionals through the development of an efficient education strategy.
1. Introduction
1. Introduction
Technological advancements have enabled shipyards to automate many aspects of shipbuilding, including welding processes. In fact, large shipyards have achieved over 70% automation of welding processes, which has led to increased efficiency and reduced costs. Despite the high level of automation, there are still manual welding processes that cannot be replaced. Manual welding is especially important for critical components of the ship, such as the hull and structural supports, where the automated machines cannot be applied.
Due to the recent boom in the shipbuilding industry and the technological demands for high quality, the demand for high-skilled welders is increasing, but the supply of such welders is still insufficient. It is not only time-consuming but also difficult to train high-skilled welders, as the current labor market tends to avoid strenuous work. Therefore, there is a need for technological solutions to cope with the difficulties in training welders. To address this issue, research is being conducted on two fronts: 1) improving the education of novice welders, and 2) formalizing the tacit knowledge of high-skilled welders into a knowledge asset of welding technology. Matsuura1) has proposed and implemented a new teaching method by implementing a technical information structure in consideration of the proficiency required for unskilled welders in order to convey the tacit knowledge of ‘sense’ of high-quality welders. Asai2) said that how to digitize and quantify the skills of high-capacity welders is an important point in fostering skilled workers and inheriting technology, and that the use of digital data is essential. Their goal is to create standard models of welding patterns that welding students can easily follow. This would enable unskilled welders to improve their welding skill in a shorter amount of time than they currently can.
Recently, machine learning has emerged as a powerful tool for improving the welding education system. By analyzing large volumes of welding process data, machine learning algorithms can uncover patterns and insights that are not immediately apparent to human observers. This technology has the potential to revolutionize the way welding-related knowledge is accumulated and utilized in training programs, leading to more effective instruction and better-trained welders.
Jung and Sim3) used the association rule algorithm of R as well as regression analysis technique to analyze the structure of power consumption and wire consumption length for a large amount of pattern variables for high-skilled welder’s welding pattern analysis. Gavidel et al.4) compared and analyzed several machine learning algorithms, such as K-nearest neighbor (KNN), support vector machine (SVM), linear discriminant analysis, and quadratic discriminant analysis, for evaluating welding process performance in gas tungsten arc welding. Unfortunately, there is still a significant lack of research dedicated to unskilled welders, and the analysis of current technology remains limited. Therefore, it is imperative that we shift our attention towards the development of a digital assetization system for welding knowledge within the welding training process, utilizing the SECI model5). The SECI model, conceptualized by Nonaka and Takeuchi, serves as a valuable framework for knowledge creation and sharing5). It describes the process of how knowledge is generated and transferred in four main stages:
  • 1) Socialization: Involves the sharing of tacit knowledge among individuals through communication and shared experiences.

  • 2) Externalization: The tacit knowledge is converted into explicit knowledge by expressing it in words or other tangible forms for sharing.

  • 3) Combination: Explicit knowledge is combined and organized within the organization to create new insights and knowledge.

  • 4) Internalization: External knowledge shared within the organization is internalized and absorbed by individuals, becoming part of their personal knowledge and experiences.

The SECI model helps understand the flow of knowledge within an organization and facilitates effective learning and knowledge sharing processes. Currently, the shipyard training center corresponds to the first socialization above, and the instructor is teaching the technology directly to the unskilled welder. As the second externalization stage, a preliminary study was conducted to extract significant differences in welding parameter data between experienced welders and unskilled welders6,7). To guide welding training within the scope of welding data implemented by skilled welders, we introduced a strategy using machine learning based on the welding pattern of skilled welders6) as shown Fig. 1.
Fig. 1
Research overview
jwj-42-1-50-g001.tif
Before moving on to the study of the combination stage, this paper proposes a practical solution for clustering-related machine learning, which evaluates data from more than 10 different welding parameters by dividing them into skilled and unskilled. Moreover, this paper introduces algorithms that can provide targeted guidance for skill improvement, enhancing the overall effectiveness of welding training programs. For this purpose, the data is collected from two groups: high- skilled welders and unskilled welders. To evaluate the performance of manual welders, clustering specific machine learning algorithms such as KNN and SVM are used, and their results are compared. These study findings suggest that welding education systems could be expanded to quickly improve the welding quality of unskilled welders.
2. Data Acquisition and Preprocessing
2. Data Acquisition and Preprocessing
This chapter outlines the welding data parameters collected from welders and explains the necessary data preprocessing for analysis. In machine learning, a common technique for extracting valuable insights from numerical data involves its transformation into ranked categorical data. This process involves assigning a rank or category to each numerical value based on its relative magnitude. By doing so, we can interpret the data more easily by machine learning algorithms, which can identify patterns and make predictions based on the categories or ranks.
2.1 Data Acquisition
2.1 Data Acquisition
We describe the analysis of welding data parameters required for performance prediction techniques. A comprehensive dataset comprising 376 data points was compiled, encompassing 179 data points from high- skilled welders and 197 data points from unskilled welders. The data collection device was configured to collect data, as seen in Fig. 2, through wired and wireless communication in a way that does not affect the welder’s work safety and convenience.
Fig. 2
Manual welding data acquisition and quality inspection
jwj-42-1-50-g002.tif
Welding experiments were conducted targeting specimen thicknesses of 4 mm and 6 mm, as well as welding positions of 1G, 2G, and 3G. The experimental conditions are summarized in Table 1.
Table 1
Category of welding specimens by welding type and position
Category jwj-42-1-50-g003.tif
1G
jwj-42-1-50-g004.tif
2G
jwj-42-1-50-g005.tif
3G
Number of specimens High-skilled 72 ea 76 ea 31 ea
Unskilled 80 ea 77 ea 40 ea
Welding Condition Steel grade: SS400
Thickness: 4 mm, 6 mm
Process: FCAW
The welding quality inspection was conducted using a magnetic particle method, with a pass rate of 261 and a fail rate of 115, representing an overall fail rate of approximately 30.59 %. The high-skilled welders group showed a 100 % pass rate, while the unskilled welders group showed a fail rate of approximately 58.38 %.
The collected welding parameters for the experiment consist of a total of 21 parameters including group, ID, current (ampere), voltage, wire speed, inertial measurement unit (IMU) sensor data, work angle, travel angle, contact tip to work distance (CTWD), and welding result, as shown in Table 2. While previous research has focused on the four variables of welding speed, working angle, travel angle, and CTWD7), we explore a broader range of variables to gain a more comprehensive understanding of the factors that influence training results.
Table 2
Experimental data overview
No Parameters Description Measurement unit
1 Time Data collection time 1/1,000 sec
2 Ampere Ampere from welding machine A
3 Voltage Voltage from welding machine V
4 Wire speed Wire feeding speed Mm/s
5 IMU Roll Rotation degree of welding torch in x-axis ° (degree)
6 Pitch Rotation degree of welding torch in y-axis
7 Yaw Rotation degree of welding torch in z-axis
8 Acceleration X Acceleration speed of welding torch in the direction of x-axis
9 Acceleration Y Acceleration speed of welding torch in the direction of y-axis ɡ (gravitational acceleration)
10 Acceleration Z Acceleration speed of welding torch in the direction of z-axis
11 Angular velocity X Angular velocity of welding torch in the direction of x-axis °/s
12 Angular velocity Y Angular velocity of welding torch in the direction of y-axis
13 Angular velocity Z Angular velocity of welding torch in the direction of z-axis
14 Magnetism X Geomagnetism of welding torch in the direction of x-axis
15 Magnetism Y Geomagnetism of welding torch in the direction of y-axis µT (microtesla)
16 Magnetism Z Geomagnetism of welding torch in the direction of z-axis
17 Work Angle Angle between the weld axis and the electrode axis ° (degree)
18 Travel Angle Angle between the electrode axis and a line perpendicular to the weld axis ° (degree)
19 CTWD Contact tip to work distance mm
20 Speed Speed at which the welding torch or gun is moved across the workpiece cm/min
21 Quality Welding test quality Pass or Fail
To prevent distortion due to data outliers, the ends of the welding specimens were excluded from the measurements8). In addition to the key parameters traditionally considered in welding-related experiments, it is becoming increasingly apparent that additional parameters are required to derive a practical and effective welding behavior. This is why recent studies have explored the use of IMU sensors to collect and analyze a wider range of welding parameters. We collected 12 additional parameters through the IMU sensor, including torch rotation (roll, pitch, and yaw) for each axis, acceleration, angular velocity, and magnetism. With the aid of these parameters, a meticulous analysis of the implicit manual skills exhibited by high-skilled welders can be conducted, thus equipping unskilled welders with the ability to closely imitate the precise hand movements of their skilled counterparts.
2.2 Data Preprocessing
2.2 Data Preprocessing
It was observed that there were missing values and extreme outliers in IMU sensor data, wire feed speed, and welding speed from the raw data of 376 collected datasets. These observations are likely due to momentary torch shaking caused by sensor malfunction and sensitivity of the speed measurement device. To mitigate the influence of extreme outliers, we employed a robust preprocessing approach. Firstly, the dataset’s median was excluded from consideration. Subsequently, we utilized Python’s RobustScaler function, which normalizes the data based on the interquartile range spanning from the 1st to the 3rd quartiles, ensuring a robust standardization process. Standard normalization effectively minimizes the influence of extreme outliers and is particularly suitable for preprocessing data with frequent measurement errors that significantly affect trends.
After standard normalization, the standard deviation of each parameter was calculated through descriptive statistics to be used for performance prediction. Standard deviation is an indicator of the degree of variation in measured values, with lower standard deviation meaning lower variability in each indicator. This is more effective than measuring variations based on averages in assessing the welding skills of a welder7). Finally, the numerical data for the standard deviation of each parameter was converted into categorical data with rankings. Well-designed categorical data can significantly increase the accuracy of classification by machine learning and artificial neural networks9) and can show the differences between the high-skilled group and the unskilled group more clearly.
All numerical data, except group, ID, and quality results, were transformed into categorical data using the Likert 7-point scale, as shown in Table 3. The Likert 7-point scale is known to provide higher accuracy than other Likert scales10) and is appropriate for showing statistical information due to its higher number of data points. Rankings were designed based on the stability of each parameter value, with higher rankings indicating higher stability, meaning smaller standard deviation values. These rankings were then converted into seven categories: Excellent, Good, Above average, Average, Below average, Poor, and Very poor. The final form of the data, converted from numerical data to categorical data with rankings, is presented in Table 4.
Table 3
Linkert 7-point scales for numerical data transformation
Range of StDev (S) Scale Likert scale
S ≤ 1.5 1 Excellent
1.5 < S ≤ 2.5 2 Good
2.5 < S ≤ 3.5 3 Above average
3.5 < S ≤ 4.5 4 Average
4.5 < S ≤ 5.5 5 Below average
5.5 < S ≤ 6.5 6 Poor
6.5 < S 7 Very poor
Table 4
Form of categorical data for performance prediction of manual welding process
Group Ampere Voltage Wire speed Roll Work angle Travel angle CTWD Quality
Master Excellent Above average Excellent Excellent Excellent Excellent Excellent Pass
Master Good Average Excellent Excellent Excellent Excellent Good Pass
Trainee Above average Average Poor Excellent Excellent Excellent Excellent Pass
Trainee Above average Below average Average Good Good Good Good Fail
3. Data Analysis
3. Data Analysis
We visualize and analyze the manually welded data by examining distribution, density, and correlation to explain how the differences between parameters determine the welding quality depending on the skill level of manual welding.
3.1 Analysis of data correlation
3.1 Analysis of data correlation
Data visualization and correlation analysis of collected manual welding parameters were performed using Python3 with NumPy, Pandas, and Seaborn modules. Fig. 3 shows a histogram-based density plot of welding quality results. The group that achieved a pass quality result exhibited a narrow range of variation and high density at specific points for parameters such as Magnetism X, Roll, Pitch, Yaw, Work angle, Travel angle, CTWD, and Speed. Additionally, this group demonstrated a consistent performance with minimal fluctuations in these parameters. In contrast, the group that did not pass quality standards had a wider range of variation for the parameters Ampere, Voltage, Wire speed, and Angular velocity X, Y, Z, indicating that they had difficulty maintaining consistent performance in these categories.
Fig. 3
Histogram-based density plot of welding parameters
jwj-42-1-50-g006.tif
The scatterplot can confirm the tendency and trend between each independent variable. As it can be seen from the scatterplot graph of Fig. 4, it can be seen that the distribution of Yaw, Work angle, and Travel angle is widely spread in the group that failed the quality test among trainees. In the group that passed the quality test, it can be seen that the fluctuation range of the Yaw, Work angle, and Travel angle is small for skilled welders. In addition, parameters that visually show the difference between the success and failure of welding results in the trainee group cannot be identified, but there is a difference in the distribution of work angle and travel angle.
Fig. 4
Scatter plot by group quality
jwj-42-1-50-g007.tif
3.2 Data correlation between three population groups
3.2 Data correlation between three population groups
Density graphs of the quality results for the high-skilled welder and welder trainee groups are shown in Fig. 5. As no quality issues were identified in the high-skilled welder group, we have categorized the results into three distinct groups: high-skilled welder-pass, welder trainee-pass, and welder trainee-fail.
Fig. 5
Histogram-based density plot of welding parameters for three groups
jwj-42-1-50-g008.tif
Fig. 5 reveals that the skilled welder-pass group demonstrated a concentrated distribution and narrow range of variation for Magnetism X, Y, Z, Roll, Pitch, Yaw, Angular velocity Z, Work angle, Travel angle, CTWD, and Speed. These parameters display a high density at specific points, suggesting that skilled welders maintain consistent and precise control over these variables to achieve high-quality welding outcomes.
Within the welder trainee-pass group, we observed that certain variables such as Ampere, Voltage, Wire speed, Roll, Pitch, Acceleration X, Y, Z, Work angle, Travel angle, CTWD, and Speed also exhibited concentrated levels of variability. Interestingly, we noted that the high-skilled welder-pass and welder trainee-pass groups shared similar narrow ranges of variation in Roll, Work angle, Travel angle, CTWD, and Speed.
The aforementioned observations highlight the variability in welding parameters between high-skilled welders and trainee welders and suggest that different factors may influence welding quality depending on the welder’s skill level. For instance, experienced welders may have established preferred values of Ampere and Voltage and may achieve high-quality welding results by precisely controlling and adjusting other parameters, such as Magnetism and Angular velocities. The high data density of welding parameters in the high-skilled welder-pass group further suggests that minimizing unnecessary movements, such as weaving and rotation of the welding torch, may also contribute to achieving high-quality welding outcomes.
Furthermore, our analysis indicates that maintaining optimal values of Ampere, Voltage, Wire speed, CTWD, and Speed, which have been extensively researched, is critical to achieving high-quality welding outcomes for the welder trainee-pass group. We also observed that most trainee welders in this group minimize unnecessary movements of the welding torch, including Roll, Pitch, and Angular velocity parameters, to improve the welding quality level. Ultimately, our findings suggest that achieving consistent and precise control over welding parameters is critical to achieving high-quality welding outcomes, regardless of the welder’s skill level.
4. Performance Evaluation by Classification
4. Performance Evaluation by Classification
Two classification algorithms in the field of machine learning were compared and analyzed to evaluate the performance of manual welders. General logistic regression analysis was also performed and used as an indicator of comparative advantage and performance between machine learning algorithms to be compared. The main goal of our study was to compare the performance of these algorithms and identify the most effective approach for analyzing the data. By conducting a rigorous analysis, we aimed to gain insights into the factors that contribute to the quality of manual welding. Our study is expected to provide valuable information for both researchers and practitioners in the field of welding and contribute to the development of more effective and efficient welding techniques.
4.1 Evaluation by logistic regression
4.1 Evaluation by logistic regression
Logistic regression is a widely used statistical technique for predictive analysis, especially when the dependent variable is binary. This method quantifies the relationship between a binary dependent variable and one or more independent variables, which can be numeric, nominal, or ordinal, using a logistic regression function. In essence, logistic regression analysis is a type of multivariate regression that investigates the relationship between a single dependent variable and multiple independent variables. In this study, we employed logistic regression to analyze the manual welding data, and the results are presented in Fig. 6. The ROC curve and confusion matrix depicted in the figure demonstrate that logistic regression achieved an accuracy of 83.186 and an F1 Score of 80.491, respectively.
Fig. 6
Experiment result of logistic regression
jwj-42-1-50-g009.tif
4.2 Evaluation by K-nearest neighbors algorithm
4.2 Evaluation by K-nearest neighbors algorithm
The K-nearest neighbors (KNN) algorithm is a widely used non-parametric classification technique due to its simplicity and high accuracy for numerical-based classification tasks11). KNN classifies data points by grouping them into the same class as the majority of their K-nearest neighbors based on a probability density estimation method. It is important to select an appropriate K value to avoid issues such as overfitting or underfitting.
In this study, we implemented KNN using Python3 and classified the welding results into pass/fail based on a classification criterion. Hyper-parameter tuning was conducted to optimize the KNN algorithm. We split the dataset into training and validation sets in a 7:3 ratio, and the algorithm’s accuracy was evaluated by varying the distance metric as a parameter adjustment for KNN. We considered three distance measurement parameters, namely Euclidean, Manhattan, and Chebyshev, to determine the K values that yielded the highest accuracy for the validation dataset within the range of 1 to 20. Euclidean measures the minimum distance between two points without considering the direction to measure similarity, while Manhattan measures the straight-line distance between coordinates to measure similarity. Chebyshev is used in limited cases where general similarity measurement methods such as Euclidean or Manhattan cannot be applied.
Table 5 presents the accuracy of the KNN algorithm with different values of K and distance metrics after hyper-parameter tuning. The results indicate that the accuracy of the algorithm is not significantly influenced by the choice of K or distance metric. The Chebyshev distance metric had a slightly lower computation time compared to the Euclidean and Manhattan metrics.
Table 5
Accuracy variance of KNN algorithm with hyper-parameter tuning
No. Metric Number of neighbors Estimated accuracy Calculation time [sec]
1 Euclidean 5 0.7965 0.0299
2 Euclidean 6 0.7965 0.0195
3 Manhattan 5 0.7965 0.0169
4 Manhattan 6 0.7965 0.0196
5 Chebyshev 5 0.7965 0.0194
6 Chebyshev 6 0.7965 0.0101
Fig. 7 illustrates the performance of the KNN algorithm with hyper-parameter tuning, displaying the receiver operating characteristic (ROC) curve and the confusion matrix. The ROC curve displays the sensitivity and specificity of the algorithm, with sensitivity on the y-axis and specificity on the x-axis. The closer the curve is to the upper left corner, the more accurate the classification is. The confusion matrix shows the accuracy of actual versus predicted classification, with an overall accuracy of 71.681 and an F1 score of 70.668. The difference between the F1 score and the algorithm accuracy may be due to the imbalanced class distribution with a ratio of approximately 3:1 between pass and fail data. Based on the F1 score value, the estimated actual accuracy of the KNN algorithm is around 70.668.
Fig. 7
Experiment result of KNN algorithm with hyper-parameter tuning
jwj-42-1-50-g010.tif
4.3 Evaluation by support vector machine
4.3 Evaluation by support vector machine
Support Vector Machine (SVM) is a widely used machine learning algorithm that can be used for binary classification problems or to create a non-probabilistic binary linear classification model for data with two categories12). To increase the accuracy of SVM, different kernels can be applied, such as linear, polynomial, or Gaussian radial basis function.
We conducted an experiment to compare the performance of SVM using different kernels. Fig. 8 shows the results of our experiment, including the accuracy, F1 score, and ROC curve values of SVM using each kernel. Our results show that the SVM model with a linear kernel achieved the highest accuracy of 87 % among the three kernels. Fig. 8b) shows that the SVM model with a polynomial kernel had the lowest accuracy of 72 %. Lastly, Fig. 8c) shows that the SVM model with a Gaussian-Radial Basis Function kernel had an accuracy of 75 %. Overall, our comparison of the three kernels suggests that the linear kernel performed the best on our dataset. However, it is important to note that the choice of kernel should be based on the specific characteristics of the dataset and the problem at hand.
Fig. 8
Experiment results of SVM algorithm with linear, polynomial, and gaussian-RBF kernels
jwj-42-1-50-g011.tif
Our analysis revealed that high-skilled welders and unskilled welders who passed the quality test were able to adjust parameters such as Pitch and Yaw effectively, while those who failed had difficulty adjusting parameters such as CTWD and Travel angle. These findings suggest that proper adjustment of these parameters is crucial in achieving high-quality welding results. Furthermore, our analysis indicated that other parameters, such as Angular velocity X, Acceleration, and Magnetism, require further detailed analysis. These parameters which are corresponding to welding torch’s method of manipulation may have a significant impact on welding quality, but their contributions may be more complex and require further investigation.
The contribution analysis of each parameter by using the SVM, which showed the highest accuracy, is presented in Table 6.
Table 6
Classification of parameters contributing to welding quality
Classification Parameters
Parameters related to pass Angular velocity X, Magnetism Z, Pitch, Yaw
Parameters related to fail CTWD, Angular velocity Y, Travel angle, Acceleration Y, Acceleration Z
4.4 Comparison results
4.4 Comparison results
The results of the comparative analysis of machine learning algorithms as well as the regression analysis for performance evaluation of manual welders are shown in Table 7 and Fig. 9. The general logistic regression analysis was used as a metric for comparing the superiority and performance of each algorithm. As shown in Table 7, the SVM algorithm demonstrates an accuracy of 87%, which is approximately 4% higher than logistic regression analysis and approximately 15% higher than the KNN algorithm. Additionally, in terms of F1 score, SVM outperforms logistic regression analysis by 5 points and KNN by 14 points.
Table 7
Comparison of three evaluation algorithms
Metric Algorithms
Logistic regression KNN SVM
F1 score 80 71 85
Accuracy 83 72 87
Confusion matrix [26  613  68] [30  725  51] [15  53   38]
ROC score 83 74 84
Fig. 9
Comparison of ROC curves of three evaluation algorithms
jwj-42-1-50-g012.tif
Moreover, in the analysis of the ROC curve, there is a negligible difference between SVM with a linear kernel and logistic regression analysis. These findings suggest that the data collected from high-skilled welders and unskilled welders exhibit a certain degree of linearity between the welding quality inspection results and welding parameters.
Therefore, through these results, we were able to confirm two things. Firstly, we observed linearity between the welding variables and welding quality inspection results through the collection and preprocessing of data from manual welders for machine learning training. Confirming linearity implies that the collected welding variables and welding results were well aligned through data preprocessing, suggesting that machine learning is likely to perform well in capturing this relationship. Secondly, among the compared algorithms, SVM with a linear kernel was determined to be the most efficient.
5. Conclusions
5. Conclusions
The field of welding is experiencing a surge in the application of cutting-edge technologies like artificial intelligence and big data analysis. Researchers are increasingly using these tools to predict welding quality by analyzing welding variables, leading to the advancement of welding automation. Despite this progress, manual welding remains a significant part of shipyard work, and the shortage of skilled welders continues to be a challenge. To address this ongoing issue, it is crucial to delve deeper into the implicit knowledge possessed by skilled welders. This can be achieved by investigating the correlation between quality and a broader range of variables and data beyond those traditionally analyzed in previous studies.
In this paper, we attempted to asset and analyze the tacit knowledge of high-skilled welders in the second stage according to the SECI model and use it for the manual welding education system and technology transfer strategy of welding trainees. We undertook a comprehensive comparative analysis of classification algorithms with the aim of assessing welding quality based on manual welding parameters, specifically focusing on torch movement parameters like the torch weaving technique. The outcomes of this analysis can be summarized as follows:
  • 1) Effective Preprocessing with the Likert Scale: We initiated our study by investigating the suitability of various preprocessing techniques. Notably, we confirmed the effectiveness of employing a 7-point Likert scale during the preprocessing stage. This approach provided a linear framework that successfully aligned the range setting with welding variables. This alignment was instrumental in training our machine learning model with the manual welding data we collected, ensuring a meaningful connection between these variables and welding quality.

  • 2) Insights from Data Visualization Analysis: Our data visualization analysis yielded insightful observations regarding the welding process. We found that the group that passed the welding quality inspection exhibited a remarkable degree of consistency in their torch movement parameters throughout the welding process. This consistency extended to crucial parameters such as Roll, Yaw, and CTWD. This finding underscores the pivotal role played by stability and uniformity in these welding process parameters when striving for high- quality welding outcomes.

  • 3) Optimal Algorithm Selection: As part of our investigation, we compared various machine learning algorithms for their efficacy in evaluating the performance of welding trainees. Remarkably, the SVM with a linear kernel emerged as the clear winner, achieving a remarkable accuracy rate of 87%. This finding firmly establishes SVM with a linear kernel as the most suitable choice for assessing the performance of welding trainees based on our dataset.

The study findings revealed that manual welding data associated with high-quality welding is strongly correlated with variables such as roll, yaw, and CTWD of the welding torch manipulation. Moreover, it was discovered that the tacit knowledge of high-skilled welders resides in their hand skills for welding torch manipulation, and it is possible to acquire this knowledge by analyzing hand skill-related data. Therefore, incorporating visual or other forms of conveying the tacit knowledge of high-skilled welders during welding education can significantly reduce the amount of time it takes for trainee welders to attain the same level of proficiency.
Based on the results of this study, we will induce training of unskilled people to the range of optimal welding variables corresponding to the three-stage combination of the SECI model. In other words, research will continue on regression analysis algorithms that can induce weaving motion variables that affect welding quality, CTWD, and progress angle to the optimal range.
Acknowledgments
Acknowledgments

This work was supported by the Industrial Technology Innovation Program (20016155, Development of human factor-based knowledge assessment system for manual welding technology) funded by the Ministry of Trade, Industry & Energy of Korea and Korea Evaluation Institute of Industrial Technology.

REFERENCES
REFERENCES

References

1. Y. Matsuura, Development of a New Welding Skill Education Method Oriented to Skill Science, J. Japan. Weld. Soc. 92(1) (2023) 27–32. https://doi.org/10.2207/jjws.92.27
[Article]
2. S. Asai, Welding Skill Education Using 3D Digital Welding Helmet with Extreme Wide-field Visualization Technology, J. Japan. Weld. Soc. 92(1) (2023) 13–21. https://doi.org/10.2207/jjws.92.13
[Article]
3. S. H. Jung and C. B. Sim, A Study on a Working Pattern Analysis Prototype using Correlation Analysis and Linear Regression Analysis in Welding Big Data Environment, J . Korea. Inst. Elect. Comm. Sci. 9(10) (2014) 1071–1078. https://doi.org/10.13067/JKIECS.2014.9.10.1071
[Article]
4. S. Z. Gavidel, S. Lu, and J. L. Rickli1, Performance analysis and comparison of machine learning algorithms for predicting nugget width of resistance spot welding joints, Int. J. Adv. Manuf. Technol. 105(9) (2019) 3779–3796. https://doi.org/10.1007/s00170-019-03821-z
[Article]
5. I. Nonaka and H. Takeuchi. The Knowledge-Creating Company:How Japanese Companies Create the Dynamics of Innovation, 1st Edition. Oxford University Press. New York, USA: (1995)

6. C. S. Song and J. H. Nam, A Study on the Derivation Method for Optimal Variable Range of Highly Skilled Welder's Manual FCAW Using Machine Learning, Proceedings of the IWJC-Korea. (2022) 171–172.

7. W. H. Ju, H. C. Ryu, K. S. Lim, and S. M. Cho, A Study on the Measuring Method of Work Parameters to Evaluate the Skill of FCAW Welding Trainee, J. Weld. Join. 38(3) (2020) 295–299. https://doi.org/10.5781/JWJ.2020.38.3.9
[Article]
8. J. Y. Park and S. H. Song, Study on the Evaluation of Welding Soundness Based on Arc Stability and Bead Quality using the Statistical Analysis of Arc Power and Arc Dynamic Resistance, J. Weld. Join. 37(6) (2019) 599–604. https://doi.org/10.5781/JWJ.2019.37.6.10
[Article]
9. E. Fitkov-Norris, S. Vahid, and C. Hand, Evaluating the Impact of Categorical Data Encoding and Scaling on Neural Network Classification Performance:The Case of Repeat Consumption of Identical Cultural Goods, Engineering Applications of Neural Networks:13th International Conference, EANN 2012, London, UK, September 20-23, 2012. Proceedings 13. Springer Berlin Heidelberg(2012) 343–352. https://doi.org/10.1007/978-3-642-32909-8_35
[Article]
10. J. Dawes, Do Data Characteristics Change According to the Number of Scale Points Used An Experiment using 5-point, 7-point and 10-point Scales, Int. J. Mark. Res. 50(1) (2008) 61–104. https://doi.org/10.1177/147078530805000106
[Article]
11. N. A. Samsudin and A. P. Bradley, Nearest Neighbour Group-based Classification, Pattern. Recognit. 43(10) (2010) 3458–3467. https://doi.org/10.1016/j.patcog.2010.05.010
[Article]
12. S. Suthaharan. In:Machine Learning Models and Algorithms for Big Data Classification, Support Vector Machine. Integrated Series in Information Systems. 36 Springer; Boston, Massachusetts, USA: (2016), p. 207–235

Go to Top