Warning: fopen(/home/virtual/kwjs/journal/upload/ip_log/ip_log_2026-03.txt): failed to open stream: Permission denied in /home/virtual/lib/view_data.php on line 100 Warning: fwrite() expects parameter 1 to be resource, boolean given in /home/virtual/lib/view_data.php on line 101 Effect of Carbon on the Solidification Cracking Behavior in the Austenitic Fe-Mn-Al-C Lightweight Steel Welds

Effect of Carbon on the Solidification Cracking Behavior in the Austenitic Fe-Mn-Al-C Lightweight Steel Welds

Article information

J Weld Join. 2025;43(5):543-551
Publication date (electronic) : 2025 October 31
doi : https://doi.org/10.5781/JWJ.2025.43.5.6
* Institute of Environmental Science and Technology, SK Innovation, Daejeon, 34124, Korea
** Division of Materials Science and Engineering, Hanyang University, Seoul, 04763, Korea
*** Extreme Materials Research Institute, Korea Institute of Materials Science, Changwon, 51508, Korea
†Corresponding author: seonghoonid@gmail.com
Received 2025 June 6; Revised 2025 June 26; Revised 2025 July 15.

Abstract

Abstract

In this study, the solidification cracking behavior was investigated in Fe-30Mn-10.5Al-xC (x = 0.7, 0.9, 1.1 wt.%) austenitic lightweight steels. To evaluate the solidification cracking susceptibility of each alloy, a longitudinal Varestraint test was conducted with an applied strain ranging from 1 to 4%. The experimental results indicate that all the austenitic lightweight steels exhibit great resistance to solidification cracking due to the beneficial effects of high Al content, as evidenced by maximum crack length (MCL) values below 380 µm, despite their high alloying element content. However, the MCL increased directly as a function of carbon content. Microstructural analysis confirmed that the increased carbon content destabilized δ-ferrite in the fusion zone during solidification, consequently accelerating the generation and propagation of cracks. In addition, excessive carbon content also led to the formation of a eutectic (Fe, Mn)3C phase along the grain boundaries during the terminal stage of solidification, resulting in a drastic increase of solidification crack susceptibility due to its low melting point. The high content of Al and C also promoted κ-carbide precipitation in the fusion zone. However, it was confirmed that κ-carbide formation had an insignificant influence in the viewpoint of solidification crack susceptibility due to its narrow precipitation temperature range. Hence, we suggest further investigation through Varestraint test with various austenitic lightweight steels to confirm the influence of some alloying elements, for understanding the phase transition behavior in welds and improving the usability of austenitic lightweight steel in the industrial fields.

1. Introduction

Owing to the increasing requirements of energy efficiency in transportation systems, advanced steels with superior mechanical characteristics have been extensively studied in various industrial fields to meet the environmental regulations1-7). Among the different alloy systems explored, the austenitic Fe-Mn-Al-C lightweight steels, covering the chemical compositional range of Fe-(15-30)Mn-(2-12)Al-(0.5-2.0)C, have been developed with pricise controlling the alloying elements because of their unique combination of advanced mechanical properties and density reduction8-10). Res- earchers have focused on the formation mechanism and usability of nano-sized κ-carbide precipitation in austenitic lightweight steels, which plays a critical role in enhancing the mechanical properties of austenitic lightweight steels with a crystal structure of (Fe, Mn)3 AlC11-13). Ley et al. suggested an optimized heat treatment process to simultaneously obtain superior strength and toughness by controlling the size of κ-carbide precipitation in Fe-30Mn-9Al-1C-1Si-0.7Mo austenitic lightweight steel14). It has been also established that the addition of alloying elements in austenitic lightweight steels directly affects the mechanical characteristics owing to the transition of thermodynamic stability of phases15-17).

As interest in austenitic lightweight steel has steadily increased, the investigation into the weldability of the Fe-Mn-Al-C alloy system has become significantly more important since welding is a crucial process in the manufacturing of products across most industrial fields. Previous studies have provided valuable insights into the metallurgical behavior of austenitic lightweight steels during welding thermal cycles. Jeong et al. investigated the influence of precipitation behavior in the heat affected zone (HAZ), where significant microstructural and mechanical transitions can occur18). Scientists also confirmed that alloy design can effectively control the precipitation behavior of κ-carbide in the HAZ19). Kim et al. reported factors affecting ductility of the austenitic Fe-30Mn-9Al-0.9C lightweight steel at elevated temperature, which could be potential risk in welding processes20). However, further information is needed to confirm the suitability of these steels for industrial applications. In particular, solidification cracking susceptibility, which can lead to critical defects and severe failures of products, should be analyzed in detail to improve the weldability of the high manganese steel system21).

Given that the Fe-Mn-Al-C alloy system contains a significant amount of alloying elements including potentially detrimental elements with respect to hot cracking, it is essential to investigate the weld solidification cracking susceptibility of austenitic lightweight steels to ensure structural safety. In the current study, we examined the weld solidification cracking susceptibility of various Fe-Mn-Al-C austenitic lightweight steels in relation to solidification behavior and microstructural characteristics. To perform the analysis, Varestraint weldability tests on Fe-30Mn-10.5Al lightweight steels with varying carbon content were carried out. Micro- structural analyses were performed using a scanning electron microscopy (SEM) and a transmission electron microscopy (TEM) to understand the relationship between microstructure and solidification cracking susceptibility in each alloy.

2. Experimental Methods

The chemical compositions of lightweight alloys used in the current study are listed in Table 1. The original ingots were manufactured using a vacuum induction melting furnace. Each ingot was homogenized at 1,200 °C for 2 hours and then hot-rolled into plates with a thickness of 13 mm prior to water quenching. The finish rolling temperature for each plate was 900 °C. After the hot-rolling, solution treatment was conducted at 1,050 °C for 2 hours and then the plates were quenched in an ice water bath.

Chemical compositions of the austenitic light-weight steel samples

To investigate the solidification cracking susceptibility of the alloys, a longitudinal Varestraint test was carried out using a machined and ground rectangular shaped specimen (127 mm × 25.4 mm × 3 mm). Autogenous gas tungsten arc welding with Ar shielding gas was performed from one side of the specimen to the other. The detailed welding conditions are listed in Table 2. During the welding process, the augment strain was applied via die block with different radius to achieve the targeted curvature, using a pneumatically actuating yoke. The applied strain, ranging from 1% to 4%, was calculated as t/2R, where the t is the thickness of specimen and R is the radius of die block22).

Welding parameters for longitudinal varestraint test

Microstructural analyses were performed using a field emission scanning electron microscope (FE-SEM, JSM-6700F, JEOL, Japan) and the transmission electron microscope (TEM, JEOL 2100, JEOL, Japan). For FE-SEM observation, specimens were prepared by mechanical polishing with SiC papers up to 2,000 grit followed by micro-polishing with 1 µm diamond suspension. The samples were then etched with a 6% nitric acid solution in ethanol, at room temperature. To conduct TEM analysis, focused ion beam (FIB, Scios, FEI, USA) sampling method was employed for site-specific observation. All the images collected in microstructural observations were utilized for detailed investigation, using a commercial image analyzing software.

3. Results and Discussion

Fig. 1 exhibits representative microstructural images of base steel in each alloy. As shown in the figure, the microstructures of base steel in experimented alloys exhibit typical austenitic characteristics, featuring angled grains with twin boundaries. The average effective austenite grain size and ferrite fraction were measured as 53.4 µm and 6.6 % in the steel A. As the carbon content increased, the austenite grain size expanded while the fraction of ferrite phase decreased. The grain size and ferrite fraction were 72.5 µm and 0.81 % in the steel B, and the steel C exhibited fully austenitic matrix with the effective grain size of 91.1 µm.

Fig. 1

Representative base steel microstructure images of the steel A, steel B, and steel C samples with yellow arrows indicating ferrite phase

Fig. 2 illustrates the transition behavior of maximum crack length (MCL) in accordance with strain in the longitudinal Varestraint test. The results indicate that the carbon content significantly influences the solidification cracking susceptibility in the Fe-30Mn-10.5 Al-xC lightweight alloys. As shown in the figure, MCL steadily increased in all specimens as the augmented strain increased. In the steel A, no crack was observed in the 1% augmented strain condition, and the MCL was measured as 88 µm in the strain condition of 4%. In the steel B, the solidification crack lengthened from 34 µm to 171 µm as applied strain increased. In the steel C, the MCL increased drastically compared to the others. It was measured from 130 µm to 373 µm in accordance with applied strain condition. While much data should be required for verification, the current results exhibit a linear relationship between the ferrite fraction of fusion zone (F) and the MCL in the strain condition of 4% (L4%) as follow:

Fig. 2

Varestraint test results of maximum crack length (MCL) at the fusion zone as a function of augmented strain in Fe-30Mn-10.5Al-xC austenitic lightweight steels

L4%=700F+52.8

It should be noteworthy that while there was evident increment of MCL values in accordance with experimental conditions. In addition, all the experimented alloys had great resistance to solidification crack susceptibility despite the large amount of alloying elements, demonstrating less susceptibility than austenitic stainless steel welds23). Yoo et al. performed a varestraint test on Fe-18Mn-0.6C-xSi alloys, which exhibited cracks exceeding 600 μm at 4% augmented strain24). In the case of Fe-15Mn-0.5C-3.5Al-xCr alloys, cracks exceeding 700 μm were observed depending on the Cr content25). Furthermore, in comparison with previous studies on austenitic stainless steel welds, the Fe-30Mn-10.5Al-xC lightweight steel demonstrates excellent resistance to solidification cracking26).

To investigate the relationship between chemical composition and solidification cracking mechanism in the experimented lightweight alloys, Fig. 3 presents SEM micrographs of fusion zone microstructure for each alloy, which were etched to reveal the distribution of the ferrite phase. According to the figures, it was confirmed that all the lightweight alloys exhibited F-A solidification mode, as the fusion zones displayed a vermicular δ-ferrite dendritic structure. The fraction of ferrite phase decreased from 19.8% (Steel A) to 5.9% (Steel B) and 2.1% (Steel C) as the carbon content increment, as indicated in the figures. It is reasonable to state that the stability of δ-ferrite is primarily influenced by the addition of aluminum, while variations in its content among different steels are generally attributed to differences in carbon content, as reported in various studies27-30). It is obvious that the microstructure of fusion zone directly affected solidification crack resistance in each alloy, as the reduction in primary δ-ferrite is one of the significant factors in accelerating crack generation and propagation. The δ-ferrite phase has not only a higher solubility for elements with low melting temperatures but also greater elongation at elevated temperatures compared to the austenite phase31-33). In addition, it was reported that F-A solidification mode reduces both the wettability of the liquid phase and the shrinkage ratio during solidification compared to the other modes34). It is also believed that the primary δ-ferrite phase has a crack reducing effect as ferrite-austenite interface energy is lower than that of austenite-austenite interface35). Consequently, it is reasonable to conclude that the high content of Al contributes to suppress overall cracking behavior, as aluminum is a strong ferrite stabilizer. It is well known that the addition of aluminum can decrease the activity and diffusivity of carbon in austenitic steel system36). It has also been reported that aluminum inhibited the formation of the eutectic phase by maintaining the liquid phase at relatively low temperatures37). Considering the metallurgical roles of high aluminum content and the associated solidification mechanism in the lightweight steels, it is evident that the increase in MCL in the Varestraint test is directly related to δ-ferrite reduction.

Fig. 3

Representative SEM micrographs showing ferrite phase of the weld in (a) steel A, (b) steel B, and (c) steel C

For a more detailed understanding of solidification cracking behavior, Fig. 4 shows a representative SEM micrograph of a crack formed in the steel C under a 4% strain condition. According to the figure, steel C exhibited enlarged cracks with a continuous secondary phase along the grain boundaries, which was observed exclusively in the steel C. The precipitation at the crack tip can be evidence of eutectic phase which widens the solidification temperature range during the welding thermal cycle. This terminal stage of solidification may be an important factor increasing solidification crack susceptibility, promoting generation and propagation of cracks along the grain boundaries38,39). In addition, the trace of κ-carbide precipitation was also observed in the austenitic phase. Considering that the temperature range of κ-carbide formation mechanism is significantly lower than that of the fusion zone solidification, it is reasonable to conclude that the effect of κ-carbide precipitation on the solidification crack susceptibility is likely negligible40-43). In other words, κ-carbide affects the metallurgical characteristics of austenitic Fe-Mn-Al-C lightweight steels only after solidification has been completed during the welding process. In the final product stage, on the other hand, the presence of κ-carbide may have a significant impact, as its formation can enhance tensile strength and hardness while reducing ductility and impact toughness. Previous study confirmed that κ-carbide can rapidly form during the welding thermal cycle in austenitic Fe-Mn-Al-C lightweight steels, leading to increased strength and toughness loss in the simulated HAZ44).

Fig. 4

Representative solidification crack appeared in the steel C with (a) low magnification showing overall crack appearance and (b) high magnification showing crack tip with κ-carbide and grain boundary precipitates

To understand the increase of solidification cracking susceptibility with respect to carbon content, Fig. 5 illustrates the results of TEM analysis for the nano-sized precipitation at the crack tip of steel C. Through the TEM micrograph and selected area electron diffraction (SAED) patterns, it was confirmed that the particles formed along the crack tip were eutectic M3C carbide45). Ishida et al. confirmed that M₃C carbide can form at elevated temperatures in various Fe-Mn-Al-C alloys46). It was also reported that the formation of M₃C carbide affects the mechanical properties of Fe-Mn- Al-C lightweight steels47). It is to say that the M3C carbide at the dendritic and grain boundaries formed due to the segregation of austenite stabilizing elements such as Mn and C during cooling thermal cycle, since the tested alloys had F-A solidification mode. As the segregation and precipitation mechanisms are inevitably accelerated by the carbon content, the temperature range of solidification during welding expands thereby cracking susceptibility increment. Lee et al. showed that the eutectic M3C precipitation causes increasing the temperature range of mushy zone, where the solid and liquid phases coexist because of its low melting point48). Similar experimental results were reported in the austenitic high manganese steels, increased solidification cracking behavior because of M3C eutectic phase formation at the boundaries in the welding process25). Therefore, considering the drastic increase of solidification cracking susceptibility from steel B to steel C, it is reasonable to conclude that the formation of eutectic phase in the fusion zone should be avoided in designing Fe-Mn-Al-C austenitic lightweight steels.

Fig. 5

(a) TEM micrograph of grain boundary precipitation obtained by FIB extraction with a SAED pattern confirming eutectic M3C phase, (b) TEM micrograph of fusion zone with a SAED pattern confirming the austenite matrix and κ-carbide precipitation

Based on the experimental results, we found that carbon content possesses significant influence on solidification crack susceptibility in the Fe-30Mn-10.5Al austenitic lightweight steels. The crack propagation mechanism can be explained by the transition in fusion zone microstructure and presence of nano-sized eutectic phase, which are caused by increasing carbon content. However, while the excessive carbon content caused negative influence on the solidification crack susceptibility, all the experimented alloys exhibited excellent hot ductility characteristics. Therefore, to improve the usability of austenitic lightweight steels in industrial fields, it is suggested that further investigation showing solidification crack susceptibility should be conducted as researchers continue to develop various types of austenitic lightweight steels with different alloying elements and manufacturing methods49-51).

4. Conclusions

In the current study, the solidification cracking susceptibilities of Fe-30Mn-10.5Al-(0.7-1.1)C alloys were evaluated via longitudinal Varestraint test. We found several insights from the experiments, summarized as follows:

  • 1) The experimental results confirmed that the Fe- 30Mn-10.5Al-xC austenitic lightweight steels commonly had a great resistance against solidification crack susceptibility in the Varestraint test, compared to austenitic stainless steels.

  • 2) While the generation and propagation of cracks were suppressed by the high content of Al, microstructural analysis confirmed that the increasing carbon content directly affected solidification crack susceptibility, causing deterioration of δ-ferrite phase and increasing MCL.

  • 3) The reason of significantly accelerated crack propagation in the steel with 1.1 wt.% C was explained by the formation of eutectic (Fe, Mn)3C phase at the grain boundary, caused continuous vulnerable grain boundary at the final stage of solidification.

  • 4) While κ-carbide particles were observed in the fusion zone microstructure, it had only negligible influence on solidification crack susceptibility due to its precipitation temperature range. However, the precipitates might have an additional effect on the product because of their mechanical characteristics.

Acknowledgments

This research is supported by the Material and Component Technology Development Program (10048157) funded by the Ministry of Trade, Industry and Energy (MOTIE, Republic of Korea).

References

1. Kang Y. J, Jeong S. H, Kang J. H, Lee C. H. Factors affecting the inclusion potency for acicular ferrite nucleation in high-strength steel welds. Metall. Mater. Trans. A 47(6)2016;:2842–2854. https://doi.org/10.1007/s11661-016-3456-0.
2. Lesch C, Kwiaton N, Klose F. B. Advanced high strength steels (AHSS) for automotive applications- tailored properties by smart microstructural adjustments. Steel Res. Int 88(10)2017;:1700210. https://doi.org/10.1002/srin.201700210.
3. Kim J. G, Enikeev N. A, Seol J. B, Abramova M. M, Karavaeva M. V, Valiev R. Z, Park C. G, Kim H. S. Superior strength and multiple strengthening mechanisms in nanocrystalline TWIP steel. Sci. Rep 8(1)2018;:11200. https://doi.org/10.1038/s41598-018-29632-y.
4. Zeng Z, Reddy K. M, Song S, Wang J, Wang L, Wang X. Microstructure and mechanical properties of Nb and Ti microalloyed lightweight δ-TRIP steel. Mater. Charact 1642020;:110324. https://doi.org/10.1016/j.matchar.2020.110324.
5. Jeong S. H, Hong S. L, Seo J. S, Choi W. H. Effect of Line-Heating on the Microstructural and Mechanical Characteristics of 320-MPa-Grade High- Strength Hull Plates. J. Weld. Join 40(4)2022;:352–3 57. https://doi.org/10.5781/JWJ.2022.40.4.8.
6. Badkoobeh F, Mostaan H, Rafiei M, Bakhsheshi- Rad H. R, Berto F. Microstructural characteristics and strengthening mechanisms of ferritic-martensitic dual-phase steels:a review. Metals 12(1)2022;:101. https://doi.org/10.3390/met12010101.
7. Jeong S. H, Hong S. L, Seo J. S, Son J. H, Joo H. G. A study on the Microstructure and Mechanical Properties of the Coarse Grain Heat Affected Zone in EH40 Grade High Strength Structural Steels. J. Weld. Join 40(5)2022;:410–415. https://doi.org/10.5781/JWJ.2022.40.5.6.
8. Moon J. O, Park S. J, Jang J. H, Lee T. H, Lee C. H, Hong H. U, Han H. N, Lee J. E, Lee B. H, Lee C. H. Investigations of the microstructure evolution and tensile deformation behavior of austenitic Fe-Mn-Al-C lightweight steels and the effect of Mo addition. Acta Mater 1472018;:226–235. https://doi.org/10.1016/j.actamat.2018.01.051.
9. Moon J. O, Ha H. Y, Kim K. W, Park S. J, Lee T. H, Kim S. D, Jang J. H, Jo H. H, Hong H. U, Lee B. H, Lee Y. J, Lee C. H, Suh D. W, Han H. N, Raabe D, Lee C. H. A new class of lightweight, stainless steels with ultra-high strength and large ductility. Sci. Rep 102020;:12140. https://doi.org/10.1038/s41598-020-69177-7.
10. Yang J, Dong H, Li P, Xia Y, Wu W, Wang B. Analysis of microstructural evolution and mechanical properties in the simulated heat-affected zone of Fe-23Mn-0.45 C-1.5 Al high-Mn austenitic steel. J. Mater. Res. Technol 202022;:1110–1126. https://doi.org/10.1016/j.jmrt.2022.07.099.
11. Lee J. E, Kim H. S, Park S. J, Moon J. O, Han H. N. Correlation between macroscale tensile properties and small-scale intrinsic mechanical behavior of Mo-added Fe-Mn-Al-C lightweight steels. Mater. Sci. Eng A 7682019;:138460. https://doi.org/10.1016/j.msea.2019.138460.
12. Chen P, Li X, Yi H. The κ-Carbides in Low- Density Fe-Mn-Al-C Steels:A Review on Their Structure, Precipitation and Deformation Mechanism. Metals 10(8)2020;:1021. https://doi.org/10.3390/met10081021.
13. Zhang J, Jiang Y, Zheng W, Liu Y, Addad A, Ji G, Song C, Zhai Q. Revisiting the formation mechanism of intragranular κ-carbide in austenite of a Fe-Mn-Al-Cr-C low-density steel. Scr. Mater 1992021;:113836. https://doi.org/10.1016/j.scriptamat.2021.113836.
14. Ley N. A, Young M. L, Hornbuckle B. C, Field D. M, Limmer K. R. Toughness enhancing mechanisms in age hardened Fe-Mn-Al-C steels. Mater. Sci. Eng A 8202021;:141518. https://doi.org/10.1016/j.msea.2021.141518.
15. Moon J. O, Park S. J, Jang J. H, Lee T. H, Lee C. H, Hong H. U, Suh D. W, Kim S. H, Han H. N, Lee B. H. Atomistic investigations of κ-carbide precipitation in austenitic Fe-Mn-Al-C lightweight steels and the effect of Mo addition. Scr. Mater 1272017;:97–101. https://doi.org/10.1016/j.scriptamat.2016.08.036.
16. Jeong S. H, Lee Y. C, Park G. T, Kim B. Y, Moon J. O, Park S. J, Lee C. H. Phase transformation and the mechanical characteristics of heat-affected zones in austenitic Fe-Mn-Al-Cr-C lightweight steel during post-weld heat treatment. Mater. Charact 1772021;:111150. https://doi.org/10.1016/j.matchar.2021.111150.
17. Ren X, Li Y, Qi Y, Wang C. Effect of Micro- Alloyed/Alloyed Elements on Microstructure and Properties of Fe-Mn-Al-C Lightweight Steel. Metals 12(4)2022;:695. https://doi.org/10.3390/met12040695.
18. Jeong S. H, Park G. T, Kim B. Y, Moon J. O, Park S. J, Lee C. H. Precipitation behavior and its effect on mechanical properties in weld heat-affected zone in age hardened FeMnAlC lightweight steels. Mater. Sci. Eng A 7422019;:61–68. https://doi.org/10.1016/j.msea.2018.10.125.
19. Jeong S. H, Park G. T, Lee C. H. Influence of Chromium Addition on the Microstructure and Mechanical Properties in the Weld of Austenitic Lightweight Steel. J. Weld. Join 43(3)2025;:242–251. https://doi.org/10.5781/JWJ.2025.43.3.2.
20. Kim B. Y, Jeong S. H, Park S. J, Moon J. O, Lee C. H. Roles of (Fe, Mn) 3 Al Precipitates and MBIP on the Hot Ductility Behavior of Fe-30Mn-9Al-0.9 C Lightweight Steels. Met. Mater. Int 252019;:1019–1026. https://doi.org/10.1007/s12540-019-00248-9.
21. Park G. T, Jeong S. H, Lee C. H. Fusion weldabilities of advanced high manganese steels:A review. Met. Mater. Int 272021;:2046–2058. https://doi.org/10.1007/s12540-020-00706-9.
22. Shankar V, Gill T. P. S, Mannan S. L, Sundaresan S. Criteria for hot cracking evaluation in austenitic stainless steel welds using longitudinal varestraint and transvarestraint tests. Sci. Technol. Weld. Joining 5(2)2000;:91–97. https://doi.org/10.1179/136217100101538074.
23. Arata Y, Matsuda F, Saruwatari S. Varestraint test for solidification crack susceptibility in weld metal of austenitic stainless steels. Trans. JWRI 3(1)1974;:79–88.
24. Yoo J. H, Han K. T, Park Y. H, Lee C. H. Effect of silicon on the solidification cracking behavior and metastable carbide formation in austenitic high Mn steel welds. Mater. Chem. Phys 148(3)2014;:499–502. https://doi.org/j.matchemphys.2014.08.053.
25. Yoo J. H, Kim B. Y, Jeong Y. D, Park Y. H, Lee C. H. Influence of Cr on weld solidification cracking in Fe-15Mn-0.5 C-3.5 Al-xCr alloys. ISIJ Int 55(1)2015;:257–263. https://doi.org/10.2355/isijinternational.55.257.
26. Lee C. H. Effect of minor elements on hot cracking susceptibility of austenitic stainless steel welds. Met. Mater 21996;:81–91. https://doi.org/10.1007/BF03025950.
27. Klueh R. L, Maziasz P. J, Lee E. H. Manganese as an austenite stabilizer in Fe-Cr-Mn-C steels. Mater. Sci. Eng A 102(1)1988;:115–124. https://doi.org/10.1016/0025-5416(88)90539-3.
28. Chen S. R, Davies H. A, Rainforth W. M. Austenite phase formation in rapidly solidified Fe-Cr-Mn-C steels. Acta Mater 47(18)1999;:4555–4569. https://doi.org/10.1016/S1359-6454(99)00334-1.
29. Phan A. T, Paek M. K, Kang Y. B. Phase equilibria and thermodynamics of the Fe-Al-C system:Critical evaluation experiment and thermodynamic optimization. Acta Mater 792014;:1–15. https://doi.org/10.1016/j.actamat.2014.07.006.
30. Lee S. J, Lee C. Y, Lee Y. K. Schaeffler diagram for high Mn steels. J. Alloys Compd 6282015;:46–49. https://doi.org/10.1016/j.jallcom.2014.12.134.
31. Arata Y, Matsuda F, Katayama S. Solidification crack susceptibility in weld metals of fully austenitic stainless Steels (Report I):Fundamental investigation on solidification behavior of fully austenitic and duplex microstructures and effect of ferrite on microsegregation. Trans. JWRI 5(2)1976;:135–151.
32. Saida K, Okabe Y, Hata K, Nishimoto K, Kiuchi K, Nakayama J. Hot cracking behaviour and susceptibility of extra high purity type 310 stainless steels. Sci. Technol. Weld. Joining 15(1)2010;:87–96. https://doi.org/10.1179/136217109X12590746472454.
33. Bang K. S, Pak S. H, Ahn S. K. Evaluation of weld metal hot cracking susceptibility in superaustenitic stainless steel. Met. Mater. Int 192013;:1267–1273. https://doi.org/10.1007/s12540-013-6019-6.
34. Lippold J. C. Welding metallurgy and weldability. John Wiley &Sons, Inc. New Jersey, USA: 2014. https://doi.org/10.1002/9781118960332.
35. Kujanpää V. P, David S. A, White C. L. Formation of hot cracks in austenitic stainless steel welds-solidification cracking. Weld. J 65(8)1986;:203s–212s.
36. Zuidema B. K, Subramanyam D. K, Leslie W. C. The effect of aluminum on the work hardening and wear resistance of Hadfield manganese steel. Metall. Trans. A 181987;:1629–1639. https://doi.org/10.1007/BF02646146.
37. Yoo J. H, Kim B. Y, Park Y. H, Lee C. H. Microstructural evolution and solidification cracking susceptibility of Fe-18Mn-0.6 C-xAl steel welds. J. Mater. Sci 50(1)2015;:279–286. https://doi.org/10.1007/s10853-014-8586-4.
38. Kou S. Welding metallurgy John Wiley &Sons, Inc. New Jersey, USA: 2003. p. 223–225. https://doi.org/10.1002/0471434027.
39. Han K. T, Yoo J. H, Lee B. K, Han I. W, Lee C. H. Effect of Ni on the hot ductility and hot cracking susceptibility of high Mn austenitic cast steel. Mater. Sci. Eng A 6182014;:295–304. https://doi.org/10.1016/j.msea.2014.09.040.
40. Burja J, Šetina Batič B, Balaško T. Kappa Carbide Precipitation in Duplex Fe-Al-Mn-Ni-C Low-Density Steel. Crystals 11(10)2021;:1261. https://doi.org/10.3390/cryst11101261.
41. Lee J. E, Kim H. S, Jeong K. J, Park S. J, Moon J. O, Kang S. G, Han H. N. Prediction of precipitation kinetics and strengthening in FeMnAlC lightweight steels. J. Mater. Res. Technol 142021;:2897–2908. https://doi.org/10.1016/j.jmrt.2021.08.094.
42. Kaltzakorta I, Gutierrez T, Elvira R, Jimbert P, Guraya T. Evolution of microstructure during isothermal treatments of a duplex-austenitic 0.66 C11. 4Mn. 9.9 Al low-density forging steel and effect on the mechanical properties. Metals 11(2)2021;:214. https://doi.org/10.3390/met11020214.
43. Jeong S. H, Moon J. O, Park S. J, Lee C. H. Effect of Cr on the Hot Ductility of Austenitic Fe- Mn-Al-C Lightweight Steel. J. Weld. Join 42(2)2024;:200–205. https://doi.org/10.5781/JWJ.2024.42.2.7.
44. Jeong S. H, Kim B. Y, Moon J. O, Park S. J, Lee C. H. Influence of κ-carbide precipitation on the microstructure and mechanical properties in the weld heat-affected zone in various FeMnAlC alloys. Mater. Sci. Eng A 7262018;:223–230. https://doi.org/10.1016/j.msea.2018.04.088.
45. Kim B. Y. Ph. D. thesis. Weldability of austenitic Fe- Mn-Al-C lightweight steels. Hanyang University. Seoul, Korea: 2020.
46. Ishida K, Ohtani H, Satoh N, Kainuma R, Nishizawa T. Phase equilibria in Fe-Mn-Al-C alloys. ISIJ Int 301990;:680–686.
47. Gutierrez-Urrutia I. Low density Fe-Mn-Al-C steels:phase structures, mechanisms and properties. ISIJ Int 61(1)2021;:16–25. https://doi.org/10.2355/isijinternational. ISIJINT-2020-467.
48. Lee J. E, Park S. W, Kim H. S, Park S. J, Lee K. H, Kim M. Y, Madakashira P. P, Han H. N. Simulation of κ-carbide precipitation kinetics in aged low-density Fe-Mn-Al-C steels and its effects on strengthening. Met. Mater. Int 24(4)2018;:702–710. https://doi.org/10.1007/s12540-018-0089-4.
49. El-Bagoury N, Moussa M. E, Ibrahim K, Ghayad I, Halfa H. Influence of Cr and Solution Treatment on Structure and Properties of New Class Lightweight Fe-Mn-Al-C Stainless Steels. Metall. Microstruct. Anal 112022;:38–58. https://doi.org/10.1007/s13632-022-00820-7.
50. Park H. K, Lee C. U, Kim K. W, Kim S. D, Jang J. H, Ha H. Y, Moon J. O, Lee C. H, Park S. J. Effect of S addition on mechanical and machinability properties in austenitic Fe-Mn-Al-C lightweight steels. Mater. Sci. Eng A 8562022;:143939. https://doi.org/10.1016/j.msea.2022.143939.
51. Zhao T, Rong S, Hao X, Wang Y, Chen C, Wang T. Effect of Nb-V microalloying on hot deformation characteristics and microstructures of Fe-Mn-Al- C austenitic steel. Mater. Charact 1832022;:111595. https://doi.org/10.1016/j.matchar.2021.111595.

Article information Continued

Table 1

Chemical compositions of the austenitic light-weight steel samples

Steel (wt.%) C Mn Al Fe
A 0.74 29.9 10.5 Bal.
B 0.92 29.8 10.4
C 1.15 29.7 10.4

Table 2

Welding parameters for longitudinal varestraint test

Welding current 100 A
Welding voltage 12 V
Travel speed 4 mm/sec
Shielding gas Argon
Flow rate of shielding gas 15 L/min

Fig. 1

Representative base steel microstructure images of the steel A, steel B, and steel C samples with yellow arrows indicating ferrite phase

Fig. 2

Varestraint test results of maximum crack length (MCL) at the fusion zone as a function of augmented strain in Fe-30Mn-10.5Al-xC austenitic lightweight steels

Fig. 3

Representative SEM micrographs showing ferrite phase of the weld in (a) steel A, (b) steel B, and (c) steel C

Fig. 4

Representative solidification crack appeared in the steel C with (a) low magnification showing overall crack appearance and (b) high magnification showing crack tip with κ-carbide and grain boundary precipitates

Fig. 5

(a) TEM micrograph of grain boundary precipitation obtained by FIB extraction with a SAED pattern confirming eutectic M3C phase, (b) TEM micrograph of fusion zone with a SAED pattern confirming the austenite matrix and κ-carbide precipitation