Warning: fopen(/home/virtual/kwjs/journal/upload/ip_log/ip_log_2026-04.txt): failed to open stream: Permission denied in /home/virtual/lib/view_data.php on line 100 Warning: fwrite() expects parameter 1 to be resource, boolean given in /home/virtual/lib/view_data.php on line 101 Improved Accuracy of Prediction of Thermal Deformation of the Stern Shaft Block Considering the Erection Process

Improved Accuracy of Prediction of Thermal Deformation of the Stern Shaft Block Considering the Erection Process

Article information

J Weld Join. 2023;41(3):195-201
Publication date (electronic) : 2023 June 30
doi : https://doi.org/10.5781/JWJ.2023.41.3.8
* Ship and Offshore Research Institute, Samsung Heavy Industry Co. Ltd, Geoje, 53261, Korea
** Department of Naval Architecture and Ocean Engineering, Pusan National University, Busan, 46241, Korea
*** The Korea Ship and Offshore Research Institute, Pusan National University, Busan, 46241, Korea
†Corresponding author: seojk@pusan.ac.kr
Received 2023 February 3; Revised 2023 April 7; Accepted 2023 May 9.

Abstract

Thermo-elasto-plastic analysis using nonlinear finite element analysis is used for predicting welding-induced structural deformation; however, its application in the prediction of welding deformation in large structures, such as ships and offshore plants, is practically impossible. Therefore, in this study, an inherent strain-based thermal deformation analysis method, which can be applied to large structures, was developed; furthermore, the inherent strain-based analysis was used for predicting the welding deformation occurring during block erection welding. However, although the tendency is somewhat similar in terms of quality, it still differs from the actual measured value in terms of quantity. In this study, a regression equation was derived by analyzing the sensitivity of the variables used in the existing method, and, subsequently, the results corresponding to the measured values were obtained; finally, the accuracy improvement for the three ships was confirmed. Therefore, using the proposed method, it is possible to improve the technology of predicting and controlling hull deformation.

1. Introduction

The ship’s shaft transfers power from the engine to the propeller and transmits the thrust obtained from the propeller to the hull. It is responsible for maneuverability among the three features of the ship, i.e. floatability, load-carrying capacity, and maneuverability’. During the shipbuilding process, if the shaft is not aligned in a straight line or experiences significant vertical displacement, it can affect the ship’s maneuverability through damage to the bush, frictional heating, lubrication system leakage, and excessive burden on engine, leading to financial losses due to repair and transportation delay. Therefore, these factors are closely analyzed and examined during the ship design and production processes.

In the shipbuilding process, the hull is constructed through a series of processes that involve welding, such as minor assembly, sub-block assembly, block assembly, and pre-erection (PE). These processes necessarily involve the residual stress and hull deformation caused by welding.

In particular, the deformation of the hull that surrounds the shaft during the hull assembly and welding processes should not exceed the allowable range. Since exceeding the range may result in a failure in shaft alignment, technology to predict the deformation under production loads is essentially required.

As for the ship’s shaft system shown in Fig. 1, the hull is completed in the PE stage before the installation of the shaft and engine in the shipbuilding stage. Even after the completion of the hull, the shaft block is continuously subjected to deformation due to the welding required for the subsequent installation of PE blocks. Deformation after block erection is confirmed by measurements and analysis. This shows that the stern block erection process is the main cause of the deformation of the shaft block. Before the insertion of the shaft into the hull, the displacement of the aft bush with respect to the center of the fore bush is an important factor that can determine the installation position of the engine. Therefore, predicting and controlling the deformation of the shaft is an essential process for the successful installation of the propulsion engine.

Fig. 1

Shaft system and deformation

For this reason, many studies have been conducted on the prediction and control of initial defects resulting from welding in steel or aluminum reinforced plate structures.

In aluminum reinforced plate structures, experimental and numerical approaches were performed to predict the initial deformation caused by welding1), and the influence of residual stress was evaluated according to the welding method2). Theoretical/experimental investigations were performed on thermoelastic behavior for the static/dynamic characteristics of thin plates under different boundary conditions3), and finite element methods were developed for numerical approaches to inherent strain4). In addition, research was conducted to determine the welding shrinkage of simplified engineering approaches to predict the interaction of structural stiffness and the final equilibrium state5).

In the case of calculations by block unit, which involve an exponential increase in the number of finite elements and boundary conditions for analysis, however, it is not easy to apply welding deformation calculations using finite elements due to the limitations in computation time and computer performance.

As such, an FE analysis method that evaluates welding deformations using the thermal strain derived from thermoelastic analysis as the boundary condition of the weld was devised to reduce the computation time in evaluating the welding deformation of large shell structures, such as ship blocks6). Afterwards, a method has been used to reduce the time and effort required for the analysis of the welding deformation of large structures and derive reliable results by entering the inherent strain information of the welding material into corresponding elements using a 1D truss element7). This is an economical and effective method for predicting the overall welding deformation of large structures.

In this study, the existing thermal deformation method was used to analyze the sensitivity of input variables related to the prediction of shaft deformation that occurs during the stern block erection process for three ships (LNGC: LNG carrier, CN: container ship, and COT: crude oil tanker). Based on the results, the characteristics of the input variables were quantified, and a simplified input variable regression equation was derived.

2. Preprocessing Technique and Variables

2.1 Preprocessing technique

Prior to welding deformation analysis, the preprocessing method for the model is shown in Fig. 2. Firstly, the necessary parts are extracted from the model for structural analysis, and the blocks are divided according to the block division diagram. 1D elements are then generated along the weld lines of the divided blocks, and necessary information is entered. The key input values are the area of the weld lines, inherent strain, and imaginary temperature7).

Fig. 2

Modeling and analysis procedure

The imaginary temperature was assumed to be 1°C because the same welding temperature is applied to all weld lines on a typical steel plate. The welding area and inherent strain are derived through calculations that consider the type and thickness of steel plates and the distance between them. Since the information on all weld lines needs to be examined, considerable time is required. As such, empirical values presented in previous studies were used, and an welding area of 2,000 mm2 was applied to transverse 1D elements and 200 mm2 to longitudinal 1D elements. The inherent strain was used as the thermal expansion coefficient, and 0.02/°C was applied.

2.2 Target variables and ranges

The analysis technique used in this study is a method that implements welding shrinkage with 1D elements using a global ship model.

The key variables of this analysis technique are the cross-sectional area, imaginary temperature, and thermal expansion coefficient entered into 1D elements6). The sensitivity of these variables was analyzed to find the optimal variable values so as to obtain the most similar analysis results to the values measured in the field. Variables that are not key variables but may potentially affect the analysis results were also added and analyzed. The variables and their respective sensitivity analysis ranges are summarized in Table 1. Sensitivity analysis was conducted by adjusting the ratio of the existing variable values. For the analysis, the ratio of the changed variable values to the original variable values was set to be between 0.25 and 2.50, which is a relatively significant and reasonable range.

Variable types and ranges of the parametric study

3. Sensitivity Analysis

3.1 Target of the sensitivity analysis

The sensitivity analysis conducted in this study was targeted at a finite element model for VLCC (Very Large Crude-oil Carrier) stern. This finite element model was modeled as shown in Fig. 3 so that it could have the same nine-step erection order as the actual shipbuilding process with a block division diagram shown in Fig. 4. The materials of the stern hull of the ship are A, AH, D, and E grade steels, which are steels for ships, but only the elastic region was considered in the analysis. Therefore, the material properties applied in the analysis are as follows:

Fig. 3

The welding sequence of FE model and weld lines

Fig. 4

Block division and erection order

  • ∙ Mass Density 7.8×10-9 ton/mm3

  • ∙ Young’s Modulus 206,000 N/mm2

  • ∙ Poisson’s Ratio 0.3

The end of the stern direction shown in Fig. 1 was selected as the observation point and its displacement in the z-direction according to the change in input variables was observed because it plays an important role in predicting the deformed shaft centerline through the distance and angle between the aft bush and the fore bush in the actual erection process and has a significant impact on determining the optimal starting point of shaft alignment. In addition, the correlation between the input variable ratio and the ratio of the z-direction maximum displacements of the aft bush was set as a sensitivity indicator to quantitatively analyze the sensitivity of each input variable.

3.2 Sensitivity analysis

For the sensitivity analysis, the welding deformation analysis was conducted using MSC Marc8) (MSC Software Corporation, 2014). In the case of variables other than the ones subjected to the sensitivity analysis, the analysis was conducted by applying the original input values (VariableOriginal in Table 1). Based on this, the correlation between the input variable ratio and the ratio of the z-direction maximum displacements of the aft bush was set as a sensitivity indicator to quantitatively analyze the sensitivity of each input variable.

3.2.1 Comparison of sensitivity results

Table 2 summarizes the slopes and coefficients of determination for each variable in Fig. 5. Since the coefficient of determination exceeded 0.95 for all variables, the linearity between the change in input values and the change in the z-direction maximum displacement within the 0.25~2.5 variable ratio range could be confirmed. It was also possible to determine which variables have a larger impact on the analysis results through the slope comparison. The sensitivity for the analysis results is shown in Fig. 6.

A comparison of gradients and coefficients of determination between target variables

Fig. 5

Non-dimensional results of the parametric study

Fig. 6

Sensitivity by variable

In this study, an attempt was made to improve the accuracy of welding deformation prediction using an empirical method. In addition, welding deformation analysis was conducted by applying five thermal expansion coefficients (variable ratios: 0.25, 0.5, 1.5, 2, and 3) to three ships (174K LNGC, 13K CN, and Suez Max COT) to derive the correlation between the ratio of thermal expansion coefficients and the ratio of z-direction maximum displacements (maximum displacement when the input thermal expansion coefficient is used / the maximum displacement when the original thermal expansion coefficient is used). Through the welding deformation analysis results and linear regression analysis, a linear relationship with a slope of 0.873, a y-intercept of 0.126, and a coefficient of determination of 0.9211 could be derived. This relationship is shown in Fig. 7 along with the welding deformation analysis results.

Fig. 7

An empirical formula between ratio of z-displacement and thermal expansion coef. ratio

3.2.2 Validation of the linear relationship

The most sensitive thermal expansion coefficient was modified through the sensitivity analysis to obtain results that are similar to the measured values. To verify the validity of the empirical method, the derived linear relationship was applied to the welding deformation analysis and compared with the measurement results and the results of the analysis that used the original thermal expansion coefficient.

The relationship was applied to three ships (174K LNGC, 13K CN, and SuezMax COT), and the results of the welding deformation analysis conducted using the derived thermal expansion coefficient for each ship are shown in Fig. 8. The coefficients attached to the existing α values were derived using the formula in Fig. 7. Since the number of blocks that constitute the stern and the timing and frequency of deformation measurements vary depending on the ship, the erection welding stages shown in Fig. 8 are expressed differently for each ship.

Fig. 8

A deduction process of new thermal expansion coef. and results of welding deformation analysis with the new coef.

In Fig. 8, it can be seen that the agreement between the welding deformation analysis results and the measured values for all ships improved when the new thermal expansion coefficient was applied compared to when the original thermal expansion coefficient was used. Although there was a tendency for slight overestimation, it was confirmed that the linear relationship derived through the regression analysis is effective in improving the accuracy of the analysis results. Table 3 summarizes the error between the measured values and the analysis results when the original thermal expansion coefficient was used for each ship (Error with α of variable ratio 1), the error when the new thermal expansion coefficient derived through the empirical method was used (Error with new α), and the improvement. Here, the improvement represents the difference between the error when the original thermal expansion coefficient is used and the error when the new coefficient is used. When the new thermal expansion coefficient was used for each ship, the error decreased by a minimum of 16.9% and a maximum of 28.2%.

A comparison of errors: established vs. new thermal expansion coefficients

3.2.3 Validation of the linear relationship

The empirical method was applied to each ship above, and it was confirmed that the use of the new thermal expansion coefficient as an input value improved the accuracy of the welding deformation analysis. Based on this result, it was deemed necessary to examine the α value, which is the currently used thermal expansion coefficient. 1.62α, which is the average of ‘New α’ shown in Table 3, was selected as a new thermal expansion coefficient applicable to all ships, and it was applied to three ships (174K LNGC, 13K CN, and SuezMax COT). When 1.62α was commonly applied to the welding deformation analysis, it was found that the agreement with the measurement results increased compared to when the original α value was used as shown in Fig. 9 and Table 4. This confirmed that the empirical method through the linear relationship and the newly applied thermal expansion coefficient of 1.62α had a significant effect on improving the validity of the welding deformation analysis results.

Fig. 9

A Results of welding deformation analysis with the new coef. of 1.62α

A comparison of errors: established vs. new thermal expansion coefficient 1.62α

Fig. 10 compares the analysis results of 13K CN when the original thermal expansion coefficient and 1.62α were used. It can be seen that the deformation of the aft bush was significantly increased. In this study, the validity was verified by modifying only the thermal expansion coefficient among the variables, but it is necessary to optimize all the variables considering their contributions in the future.

Fig. 10

A comparison of z-displacement contour plot at 4th welding sequence

4. Conclusions

This study aimed to improve the effectiveness of the existing inherent strain-based welding deformation prediction technique during the construction of the shaft, and the following conclusions were drawn.

  • 1) Sensitivity analysis was conducted on the input variables of the existing welding deformation prediction technique, and it was confirmed that sensitivity to the thermal expansion coefficient of the weld joint is high. Based on the welding deformation analysis results and linear regression analysis, a linear relationship between the thermal expansion coefficient of the weld joint and the z-direction maximum displacement was derived.

  • 2) When the linear relationship was applied to the welding deformation analysis for each ship, the error between the analysis results and the measured values decreased by up to 28.2%. When a thermal expansion coefficient of 1.62α was applied to the welding deformation analysis for each ship, the error between the analysis results and the measured values decreased by up to 39.4%.

  • 3) This study attempted to reduce the error with the measured values by modifying the most sensitive factor through sensitivity analysis. Since actual deformation is caused by interactions among multiple factors, further research is required on such interactions.

References

1. Paik J. K, Kim B. J, Sohn J. M, Kim S. H, Jeong J. M, Park J. S. On Buckling Collapse of a Fusion-welded Aluminum-stiffened Plate Structure:An Experimental and Numerical Study. J. Offshore Mech. Arct. Eng 134(2)2012;:021402. https://doi.org/10.1115/1.4004511.
2. Park J, An G, Kim D. Residual Stress and Defor- mation Characteristics by FSW and SAW of Wear Resistant Steel. J. Weld. Join 40(2)2022;:133–140. https://doi.org/10.5781/JWJ.2022.40.2.4.
3. Abdul-Majeed W. Buckling &Dynamics of Thermo- elastic Plates, 1st edition. LAP LAMBERT Academic Publishing London, United Kingdom: 2011. p. 106–194.
4. Ueda Y, Murakawa H, Ma N. Welding Deformation and Residual Stress Prevention, 1st edition. Butterworth- Heinemann Oxford, United Kingdom: 2012. p. 169–207.
5. Kim J. H, Yu S, Yi M, Seo J. Secondary Thermal Deformation Characteristics of Stiffened Plate Exposed to Fire. J. Weld. Join 40(5)2022;:385–392. https://doi.org/10.5781/JWJ.2022.40.5.3.
6. Ha Y. A study on weldment boundary condition for elasto-plastic thermal distortion analysis of large welded structures. J. Weld. Join 29(4)410–415. https://e-jwj.org/journal/view.php?number=1676376.
7. Yi M. S, Park J. S, Seo J. K. A novel pre-processing modelling method for the finite element analysis of the thermal deformation of large structures in the erection stage. Ocean. Eng 266(4)2022;:112891. https://doi.org/10.1016/j.oceaneng.2022.112891.
8. Online User's Guide(2014) MSC Software Corporation California, USA https://simcompanion.hexagon.com/customrs/s/article/ marc-2014-2-user-s-guide-doc10799.

Article information Continued

Fig. 1

Shaft system and deformation

Fig. 2

Modeling and analysis procedure

Table 1

Variable types and ranges of the parametric study

Variable VariableChanged / VariableOriginal
Cross-sectional area of longitudinal truss element 0.25 - 0.50 - 1.00 - 1.50 - 2.00 - 2.50 unit: mm2/mm2 (VariableOriginal = 200 mm2)
Cross-sectional area of transverse truss element 0.25 - 0.50 - 1.00 - 1.50 - 2.00 - 2.50 unit: mm2/mm2 (VariableOriginal = 2,000 mm2
Imaginary temperature 0.25 - 0.50 - 1.00 - 1.50 - 2.00 - 2.50 unit:°C/°C (VariableOriginal = 1.0°C)
Thermal expansion coef. 0.25 - 0.50 - 1.00 - 1.50 - 2.00 - 2.50 unit:°C/°C (VariableOriginal = -0.02/°C)
Steel density 0.25 - 0.50 - 1.00 - 1.50 - 2.00 - 2.50 unit: (ton/mm3)/ (ton/mm3) (VariableOriginal = 7.80×10-9 ton/mm3)
Support stiffness 0.25 - 0.50 - 1.00 - 1.50 - 2.00 - 2.50 unit: N/N (VariableOriginal = 467,700 N)

Fig. 3

The welding sequence of FE model and weld lines

Fig. 4

Block division and erection order

Table 2

A comparison of gradients and coefficients of determination between target variables

Variable Gradient Coefficient of determination
Longitudinal truss area 0.099 mm2/mm2 0.999
Transverse truss area 0.649 mm2/mm2 0.993
Steel density 0.132 ton/mm3/ton/mm3 0.973
Support stiffness N/A N/A
Imaginary temperature 0.831°C/°C 0.999
Thermal expansion coef. 0.840 1/°C/1/°C 0.999

Fig. 5

Non-dimensional results of the parametric study

Fig. 6

Sensitivity by variable

Fig. 7

An empirical formula between ratio of z-displacement and thermal expansion coef. ratio

Fig. 8

A deduction process of new thermal expansion coef. and results of welding deformation analysis with the new coef.

Table 3

A comparison of errors: established vs. new thermal expansion coefficients

Type 174K LNGC 13K CN Suez Max COT
Error with α of variable ratio 1(%) 33.4 42.0 30.3
New α (/°C) 1.54 α 1.83 α 1.50 α
Error with new α (%) 5.2 14.5 13.4
Improvement (%) 28.2 27.5 16.9

Fig. 9

A Results of welding deformation analysis with the new coef. of 1.62α

Table 4

A comparison of errors: established vs. new thermal expansion coefficient 1.62α

Type 174K LNGC 13K CN Suez Max COT
Error with α of variable ratio 1 (%) 33.4 42.0 30.3
Error with α of 1.62α (%) 7.5 2.6 22.2
Improvement (%) 25.9 39.4 8.1

Fig. 10

A comparison of z-displacement contour plot at 4th welding sequence