Warning: fopen(/home/virtual/kwjs/journal/upload/ip_log/ip_log_2022-10.txt): failed to open stream: Permission denied in /home/virtual/lib/view_data.php on line 88 Warning: fwrite() expects parameter 1 to be resource, boolean given in /home/virtual/lib/view_data.php on line 89 A Study of Transient Liquid Phase Bonding Using an Ag-Sn3.0Ag0.5Cu Hybrid Solder Paste

A Study of Transient Liquid Phase Bonding Using an Ag-Sn3.0Ag0.5Cu Hybrid Solder Paste

Ag-Sn3.0Ag0.5Cu Hybrid Solder Paste를 이용한 천이액상 확산 접합 연구

Article information

J Weld Join. 2021;39(4):376-383
Publication date (electronic) : 2021 August 23
doi : https://doi.org/10.5781/JWJ.2021.39.4.5
* Department of Advanced Materials Engineering, Chungbuk National University, Cheongju, 28644, Korea
** Welding and Joining R&D Group, Korea Institute of Industrial Technology (KITECH), Incheon, 21999, Korea
Corresponding author: jwyoon@chungbuk.ac.kr
Received 2021 July 20; Revised 2021 August 2; Accepted 2021 August 6.

Abstract

The feasibility of transient liquid phase (TLP) bonding technology for high-temperature endurable power electronics packaging has been evaluated in this study. An Ag-Sn3.0Ag0.5Cu hybrid solder paste was fabricated and used as a bonding material. The bonding reactions between chip/substrate and hybrid solder paste and die shear strengths of the TLP-bonded joints were evaluated during conventional soldering and vacuum soldering processes. Compared to the conventional soldering, the vacuum-soldered joints had fewer voids and relatively good metallurgical microstructures. After TLP bonding, (Cu,Ni)6Sn5, Ag3Sn, and Cu6Sn5 intermetallic compounds formed at the chip interface, in the middle of the joint, and at the bottom interface, respectively. It was confirmed that the vacuum soldering process could create good interfacial uniformity with minimal voids in the Si chip/ceramic substrate joints. The formation of voids during TLP bonding significantly affected the mechanical shear strength of the TLP-bonded joints. The vacuum-soldered joints had high shear strength values of approximately 40 MPa. To ensure the high joint strength and long-term reliability of Sn-based TLP-bonded joints, critical void control in the joints is needed.

1. Introduction

The 21st century has witnessed an unprecedented level of interest in new and renewable energy such as eco-friendly vehicles and PV or wind power generation while reducing the use of fossil fuels, driven by changes in the public awareness of global environmental pollution and the recent implementation of carbon neutrality and energy efficiency policies. In particular, in the field of transportation, there has been an explosive surge of interest in electric vehicles (EVs) and hydrogen fuel cell electric vehicles (FCEVs). These eco-friendly vehicles use battery, power conversion systems, and motor systems as key components, and significant growth in relevant industries is expected1). In particular, the power modules in the inverter system, contains power semiconductors, which plays the role of converting the DC current of the battery into AC current for driving the motor. For these power semiconductors, a high level of reliability is required due to the conditions in driving eco-friendly vehicles, such as high operating temperatures and exposure to harsh environments for a long time2).

To date, for bonding of chips and modules of these power semiconductors, conventional soldering methods using high-Pb solder and Pb-free Sn-Ag-Cu solder alloys have been mainly employed3,4). However, in order to achieve the reliable operational performance of power modules under high temperature over 200 ℃ following the upcoming introduction of silicon carbide (SiC) devices, the chip bonding process with Sn-based solder alloys has come to a limitation. In addition, some solder alloys containing Pb, which can be used in high-temperature environment, still have the environmental problems as obstacles5). For this reason, in recent years, there has been active research on alternative high-temperature endurable bonding methods such as sinter bonding technology using Ag or Cu powder and transient liquid phase (TLP) bonding technology with low melting point bonding material6-13). In particular, the TLP bonding method uses a low-melting-point metal material such as Sn and In to form the high-melting-point intermetallic compounds (IMCs) showing stable properties even at high temperatures. Because the method has a relatively low process temperature and pressure as well as excellent durability at high temperatures, it has been actively investigated using combinations of various metals14-18). In this study, as basic research on TLP bonding technology, hybrid solder paste was fabricated with Ag and Sn-3.0Ag-0.5Cu solder alloys, and the changes in the microstructure and mechanical strength in solder joints were examined according to the change of TLP bonding process, and through analysis of the correlations, the future applicability of TLP bonding method was discussed.

2. Methods

In this experiment, micro Ag paste (Microbond ASP 295, Heraeus, Singapore) and Sn-3.0Ag-0.5Cu solder paste (Senju Metals, Japan) were used for the fabrication of the bonding paste. In the case of Ag paste, the Ag metal content was approximately 88%, and the average particle size was around 20 μm. Also, type-5 (average particle size 15-25 um) paste was used for the solder paste. First, a hybrid paste of Ag paste and solder paste with a weight ratio of 1:2 was prepared. For uniform mixing of the two types of pastes, a revolution-rotation mixer was used under a vacuum atmosphere condition. Fig. 1 shows the schematic diagram of the fabricated paste before and after mixing. The substrate used for the power semiconductor chip bonding process was a direct bond copper (DBC) ceramic substrate with a size of 10 × 10 × 0.98 mm, in which a sandwich structure with Cu/96% Al2O3/Cu laminates was used. The thicknesses of the ceramic layer and the copper layer were 380 μm and 300 μm, respectively. The fabricated paste was screen-printed on the DBC substrate by using a 304 stainless steel metal mask with a thickness of 50 μm. The size of the opening of the mask was 3 × 3 mm. For the TLP chip bonding process, a 3 mm × 3 mm Si dummy chip laminated with 0.1 ㎛ Ti\0.1 ㎛ Al\0.2 ㎛ Ti\1 ㎛ Ni \0.2 ㎛ Ag layer was used. These dummy chips were placed on the printed paste. Fig. 2 shows a schematic diagram of a chip/ paste/DBC substrate sample in the process of paste printing and chip attachment. Next, the TLP bonding process was performed using SMT reflow scope. The peak temperatures used in the bonding process were 245, 260, and 275 ℃, respectively, and the bonding process was performed at the peak temperature for approximately 40 seconds. The reflow temperature profile used in this study is shown in Fig. 3. In addition, a vacuum reflow process was performed for comparison with the air reflow process, and the bonding process was performed using a vacuum reflow machine (SRO 70x, ATV Technologie GMBH, Germany). Fig. 4 shows the reflow temperature profile used in the vacuum reflow process. As can be seen in the figure, the vacuum reflow process was performed with a vacuum atmosphere and formic acid, and the peak temperature was 250 ℃

Fig. 1

Schematics of paste fabrication, (a) before and (b) after mixing

Fig. 2

Schematics of paste printing and chip attachment

Fig. 3

Temperature profiles used in reflow process

Fig. 4

Temperature profile used in vacuum reflow process

In the sample completed with the bonding process, for evaluation of defects such as voids formed in the joints, non-destructive analysis was performed using X-ray equipment (XSCAN-H160-OCT, XAVIS, KOREA). After completing the TLP bonding process using the fabricated paste, the sample was mounted using epoxy material, and polishing was performed for metallurgical analysis of the cross section. The microstructure and bonding interface of each sample were analyzed using a field emission scanning electron microscope (FE-SEM, INSPECT F, FEI, USA) and an energy dispersive X-ray spectroscope (EDX). To evaluate the mechanical properties of TLP bonding samples, die shear testing was performed using a shear tester (Dage4000, Nordson DAGE, UK). In terms of the shear testing conditions used in this experiment, a shear speed of 200 μm/s and a shear height of 100 μm were used (Fig. 5). For evaluation of the die shear strengths, shear testing was performed on a total of 10 joint samples, and the fracture surfaces were analyzed after the shear testing.

Fig. 5

Schematic of die shear testing

3. Experimental results

Bonding was performed with different bonding processes to evaluate the bonding characteristics of the fabricated Ag-Sn3.0Ag0.5Cu hybrid paste, and Fig. 6 shows the OM images of the bonding sample after the conventional air reflow and vacuum reflow bonding process. As shown in the figure, for the joint sample completed with the conventional air reflow process, the surface of the DBC copper metal layer was oxidized and discolored. On the other hand, in the case of the bonded joint samples from the vacuum reflow process, suppression of the surface oxidation was confirmed. The formic acid (HCOOH) typically used during the vacuum reflow process has a boiling point of approximately 101 ℃, and it reduces metal oxides as shown in the following equations. Below is a reaction formula in which two types of copper oxides (Cu2O, CuO) are reduced by reaction with formic acid.

Fig. 6

OM images of (a) air reflowed and (b) vacuum reflowed samples

Cu2O + 2HCOOH → Cu(COOH)2 + Cu + H2O

CuO + 2HCOOH → Cu(COOH)2 + H2O

Cu(COOH)2 → Cu + 2CO2 + H2

Fig. 7 shows the non-destructive X-ray analysis images of the bonded joints under various bonding conditions and color images adjusted for these analyzed images using an image software tool. As shown in the figure, no interfacial delamination or non-bonding area was observed at the joint interface, but in the case of the sample bonded by the conventional air reflow process, the presence of a relatively large number of voids was confirmed in the joints regardless of the bonding temperature. On the contrary, in the case of samples bonded by the vacuum reflow process, the formation of quality joints was confirmed without significant defects.

Fig. 7

X-ray images and corresponding adjusted images by image tool software of bonded joints under various conditions

Fig. 8 shows the SEM images of the Si chip/DBC joint interface bonded by the air reflow process at 245 ℃ peak temperature. The SEM images of the chip interface, the middle of the joint (bonding layer), and the DBC joint in the entire joint area are presented by location along with a schematic diagram, respectively. During the bonding reaction, Ag, which is the final metal layer of chip metallization, was all dissolved by reaction with the solder to form a compound phase inside the solder, and the reaction with Ni, the subsequent metal layer, was confirmed. Through the series of reactions, it was confirmed that the (Cu,Ni)6Sn5 IMC layer containing Ni was formed at the chip joint interface (Fig. 8(a)). As a result of observing the central part of the joint (bonding layer), it was confirmed that Ag3Sn IMC, a compound of Ag and Sn, was formed and uniformly distributed due to Ag added in the Sn-3.0Ag- 0.5Cu solder (Fig. 8(b)). As a result of analyzing the lower DBC substrate joint, formation of a Cu6Sn5 IMC layer at the interface was confirmed due to the reaction between the Cu layer of the DBC substrate and the solder. Also, due to the added Ag, the additional formation of Ag3Sn IMC on the Cu6Sn5 IMC layer was confirmed (Fig. 8(c)). Fig. 9 and Fig. 10 show SEM images of the Si chip/DBC joints bonded by the air reflow process at peak temperatures of 260 and 275 ℃, respectively. Compared with the result of 245 ℃ in Fig. 8, the growth in the size and thickness of the IMC formed at some joint interfaces was observed, but no significant difference was observed, on the whole. Therefore, in this study, it was confirmed that the difference in the reflow peak temperature by 15 ℃ did not have a significant impact on the microstructure of the joints.

Fig. 8

Cross-sectional SEM images of a Si chip/bonding layer/DBC joint (peak reflow temperature: 245 ℃)

Fig. 9

Cross-sectional SEM images of a Si chip/bonding layer/DBC joint (peak reflow temperature: 260 ℃)

Fig. 10

Cross-sectional SEM images of a Si chip/bonding layer/DBC joint (peak reflow temperature: 275 ℃)

Fig. 11 shows the SEM images for each location of the Si chip/DBC joint bonded by the vacuum reflow process. As a result of the composition analysis using EDX, that the types of compounds observed at the chip interface, the middle of the joint (bonding layer) and the DBC joint were confirmed to be identical to the compounds of the samples bonded through the air reflow process. However, overall, the formations of coarse (Cu,Ni)6Sn5, Ag3Sn and Cu6Sn5 IMCs were confirmed in the joints and bonding layer, respectively.

Fig. 11

Cross-sectional SEM images of a Si chip/bonding layer/DBC joint reflowed under a vacuum condition

For evaluation of the effect of bonding process parameters on the mechanical strength of joints bonded through conventional reflow and vacuum reflow processes, die shear testing was performed, and the results are presented in Fig. 12. The shear test results confirmed that the sample bonded by the air reflow process had a shear strength of approximately 20 MPa regardless of the change in the peak temperature. On the other hand, in the case of joints bonded by the vacuum reflow process, the bonding strength was approximately twice that of the air reflow process with an average shear strength value of approximately 40 MPa.

Fig. 12

Variation of die shear strength with reflow conditions

To investigate the cause of the significant difference in die shear strength testing result, the fracture surfaces were analyzed after shear testing, and the results are presented in Fig. 13. In the case of the sample bonded by the air reflow process (Fig. 13(a)-(c)), after shear testing, fracture mainly occurred at the chip interface, and the presence of many voids was confirmed on the fracture surface. On the other hand, in the case of joint samples bonded through the vacuum reflow process (Fig. 13(d)), fracture at the chip interface was also confirmed after shear testing, as in the case of the conventional reflow process, but the no significant presence of voids on the fracture surface was confirmed. Considering these results, it was confirmed that the amount and size of voids in the joints created after the different reflow bonding processes used in this study had a significant effect on joint strength. The result of this difference in shear strength (Fig. 12) was consistent with the observation result for the voids in the joints (Fig. 7) according to the difference in the bonding process described above and a schematic diagram outlining these results is presented in Fig. 14. Although the conditions such as process temperature and holding time used in this study are not exactly the same between the air reflow and vacuum reflow processes, in general, as can be seen in Fig. 4, in the vacuum reflow process, the vacuum and formic acid are alternately applied 2-3 times at the initial stage, and thus the oxides formed on the samples are reduced and removed and there is also a process of increasing the degree of vacuum. In addition, even when the process is maintained at the peak temperature, the degree of vacuum is increased again to remarkably reduce the voids present in the molten solder and joints. For this reason, compared to the conventional air reflow process, the vacuum reflow process takes a rather long time. On the other hand, in the air reflow process, the voids present in the joint are not spontaneously released during the metallurgical reaction of the molten solder alloys between the chip and the substrate metal. In addition, since a typical size of the power semiconductor chips has an area of ​​several millimeters to approximately 10 millimeters in width and length, the natural removal of voids in the molten solder becomes more difficult. In addition, the action of formic acid used in the vacuum reflow process reduces the oxides present in the sample as described above, and the combination of the action of formic acid and the vacuum atmosphere served to significantly reduce voids in the joints. According to the results of a previous study, in the case of Cu-Sn TLP bonding joint, high shear strength of approximately 50 MPa was obtained by minimizing joint voids and inducing the reaction of Cu3Sn compound formation9). Also, as a result of shear testing, shear failure along the chip interface was reported. With the Sn-based TLP bonding, further expansion of its application is expected in electric vehicles and high-temperature-endurable electronic components and modules after undergoing sufficient tests on the reliability due to its advantages as a low-cost, high-temperature-endurable bonding material. Therefore, in this study, basic research on Sn-based TLP bonding was performed to evaluate metallurgical and mechanical properties in the joints according to reflow process parameters for the application as a high-temperatureendurable bonding material. When the TLP bonding process is performed using Sn-based low-melting point metals and alloys, a vacuum reflow process is recommended to ensure joint strength and long-term reliability, and more tightened control of joint voids is imperative. In the future, more in-depth and detailed further studies are needed.

Fig. 13

Fracture surfaces of joints bonded under various conditions

Fig. 14

Schematics of fracture sites after shear testing, (a) air reflow sample and (b) vacuum reflow sample

4. Conclusion

In this study, as basic research to examine the applicability of TLP bonding in power semiconductor modules endurable in a high-temperature environment, a hybrid solder paste using silver (Ag) and Sn-3.0Ag-0.5Cu solder materials was fabricated, and evaluation of changes in microstructure and mechanical strength was performed according to the application of different types of TLP bonding processes, and the following conclusions were derived.

  • 1) In the case of joint samples bonded by the vacuum reflow process, formic acid played a role of metal oxides reduction, and considerable suppression of the surface oxidation of the substrate was confirmed. As a result of non-destructive X-ray analysis of the joints, the presence of many voids in the joints was confirmed in the case of the sample bonded by the air reflow process, but with the vacuum reflowed sample, the formation of a relatively good interfacial uniformity without voids was confirmed.

  • 2) The analysis of the cross-sections of the joints confirmed that (Cu,Ni)6Sn5, Ag3Sn and Cu6Sn5 IMCs were formed at the chip interface, middle of the joint and DBC interface at the bottom, respectively, regardless of process parameters.

  • 3) As a result of evaluating the mechanical strength of the joints through die shear testing, in the case of joints bonded by the vacuum reflow process, the average shear strength value was approximately 40 MPa, and this value was approximately 2 times higher than that of the air reflow process. It was confirmed that the amount and size of voids created inside the joint after the bonding process had a significant impact on the joint strength.

  • 4) In the future, when the TLP bonding process is performed using Sn-based low-melting point metals and alloys, more stringent control of joint voids under vacuum reflow atmosphere is required to ensure high joint strength and long-term reliability, and in this regard, further systematic optimization study is thought to be necessary.

Acknowledgments

This research was partly supported by the research grant of the Chungbuk National University in 2020 and Korea Institute for Advancement of Technology(KIAT) grant funded by the Korea Government(MOTIE) (P0008458, The Competency Development Program for Industry Specialist).

References

1. Matallana A, Ibarra E, López I, Andreu J, Garate J.I, Jordà X, Rebollo J. Power module electronics in HEV/EV applications:New trends in wide-bandgap semiconductor technologies and design aspects. Renew. Sust. Energ. Rev 1132019;:109264. https://doi.org/10.1016/j.rser.2019.109264.
2. Yoon J. W, Bang J. H, Ko Y. H, Yoo S, Kim J. K, Lee C. W. Power module packaging technology with extended reliability for electric vehicle applications. J. Microelectron. Packag. Soc 21(4)2014;:1–13. http://dx.doi.org/10.6117/kmeps.2014.21.4.001.
3. Ciappa F, Dugal M. Study of thermal cycling and temperature aging on PbSnAg die attach solder joints for high power modules. Microelectron. Reliab 542014;:1856–1861. http://dx.doi.org/10.1016/j.microrel.2014.08.001.
4. Lee B. S, Ko Y. H, Bang J. H, Lee C. W, Yoo S, Kim J. K, Yoon J. W. Interfacial reactions and mechanical strength of Sn-3.0Ag-0.5Cu/Ni/Cu and Au-20Sn/Ni/Cu solder joints for power electronics applications. Microelectron. Reliab 712017;:119–125. https://doi.org/10.1016/j.microrel.2017.03.011.
5. Son J, Kim M, Yu D. Y, Ko Y. H, Yoon J. W, Lee C. W, Park Y. B, Bang J. Thermal aging characteristics of Sn-xSb solder for automotive power module. J. Weld. Join 35(5)2017;:38–47. https://doi.org/10.5781/JWJ.2017.35.5.6.
6. Lee B. S, Back J. H, Yoon J. W. Effect of sintering conditions on microstructure and mechanical strength of Cu micro-particle sintered joints for high-power semiconductor module applications. J. Weld. Join 37(2)2019;:26–34. https://doi.org/10.5781/JWJ.2019.37.2.5.
7. Byun Y. H, Jeong C. M, Yoon J. W, Kim C. H, Kim C. S, Lee B. W, Booh S. W, Chung U. I. A novel and simple fabrication technology for high power module with enhanced thermal performance. Proc. 8th IEEE Vehicle Power and Propulsion Conference (VPPC) 2012;:1070–1073. https://doi.org/10.1109/VPPC.2012.6422503.
8. Li J. F, Agyakwa P. A, Johnson C. M. Interfacial reaction in Cu/Sn/Cu system during the transient liquid phase soldering process. Acta Mater 592011;:1198–1211. https://doi.org/10.1016/j.actamat.2010.10.053.
9. Lee B. S, Yoon J. W. Cu-Sn intermetallic compound joints for high-temperature power electronics applications. J. Electron. Mater 472018;:430–435. https://doi.org/10.1007/s11664-017-5792-2.
10. Yoon J. W, Jeong S. E. Transient liquid phase sinter bonding with Tin-Nickel micro-sized powders for EV power module applications. J. Microelectron. Packag. Soc 28(2)2021;:71–79. https://doi.org/10.6117/kmeps.2021.28.2.071.
11. Lee B. S, Yoon J. W. Die-attach for power devices using the Ag sintering process:Interfacial microstructure and mechanical strength. Met. Mater. Int 232017;:958–963. https://doi.org/10.1007/s12540-017-6908-1.
12. Yoon J. W, Back J. H. Effect of sintering conditions on the mechanical strength of Cu-sintered joints for high-power applications. Materials 112018;:2105. https://doi.org/10.3390/ma11112105.
13. Siow K. S. Mechanical properties of nano-silver joints as die attach materials. J. Alloys Compd 5142012;:6–19. https://doi.org/10.1016/j.jallcom.2011.10.092.
14. Yoon J. W, Bae S, Lee B. S, Jung S. B. Bonding of power device to ceramic substrate using Sn-coated Cu micro paste for high-temperature applications. Appl. Surf. Sci 5152020;:146060. https://doi.org/10.1016/j.apsusc.2020.146060.
15. Liu J, Wang K, Yu F, Hang C, Fu X, Chen H, Li M. A paste based on Cu@Sn@Ag particles for die attachment under ambient atmosphere in power device packaging. J. Mater. Sci. Mater. Electron 312020;:1808–1816. https://doi.org/10.1007/s10854-019-02697-9.
16. Sun L, Zhang Y, Zhang L, Chen C.P. Reliability and strength of Cu-Sn0.5CuZnAl-Cu TLP bonded joints during thermal cycling. J. Mater. Sci. Mater. Electron 322021;:19264–19274. https://doi.org/10.1007/s10854-021-06446-9.
17. Jeong S. E, Jung S. B, Yoon J. W. Fast formation of Ni-Sn intermetallic joints using Ni-Sn paste for high-temperature bonding applications. J. Mater. Sci. Mater. Electron 312020;:15048. https://doi.org/10.1007/s10854-020-04068-1.
18. Fujino M, Narusawa H, Kuramochi Y, Higurashi E, Suga T. Transient liquid-phase sintering using silver and tin powder mixture for die bonding. Japan J. Appl. Phys 552016;:04EC14. https://doi.org/10.7567/JJAP.55.04EC14.

Article information Continued

Fig. 1

Schematics of paste fabrication, (a) before and (b) after mixing

Fig. 2

Schematics of paste printing and chip attachment

Fig. 3

Temperature profiles used in reflow process

Fig. 4

Temperature profile used in vacuum reflow process

Fig. 5

Schematic of die shear testing

Fig. 6

OM images of (a) air reflowed and (b) vacuum reflowed samples

Fig. 7

X-ray images and corresponding adjusted images by image tool software of bonded joints under various conditions

Fig. 8

Cross-sectional SEM images of a Si chip/bonding layer/DBC joint (peak reflow temperature: 245 ℃)

Fig. 9

Cross-sectional SEM images of a Si chip/bonding layer/DBC joint (peak reflow temperature: 260 ℃)

Fig. 10

Cross-sectional SEM images of a Si chip/bonding layer/DBC joint (peak reflow temperature: 275 ℃)

Fig. 11

Cross-sectional SEM images of a Si chip/bonding layer/DBC joint reflowed under a vacuum condition

Fig. 12

Variation of die shear strength with reflow conditions

Fig. 13

Fracture surfaces of joints bonded under various conditions

Fig. 14

Schematics of fracture sites after shear testing, (a) air reflow sample and (b) vacuum reflow sample