Warning: fopen(/home/virtual/kwjs/journal/upload/ip_log/ip_log_2026-06.txt): failed to open stream: Permission denied in /home/virtual/lib/view_data.php on line 100 Warning: fwrite() expects parameter 1 to be resource, boolean given in /home/virtual/lib/view_data.php on line 101 Investigation of Single Pass Welding of Thick AH36 Steel Plates in a Square Groove Butt Joint Configuration During AC-GMAW

Investigation of Single Pass Welding of Thick AH36 Steel Plates in a Square Groove Butt Joint Configuration During AC-GMAW

Article information

J Weld Join. 2020;38(3):254-262
* Department of Naval Architecture and Ocean Engineering, Chungnam National University, Daejeon, 34134, Korea
** Department of Nuclear and Quantum Engineering, KAIST, Daejeon, 34141, Korea
Corresponding author : hchung@cnu.ac.kr
Received 2020 February 05; Revised 2020 March 25; Accepted 2020 April 21.

Abstract

This study was performed to investigate the AC-GMAW process for joining of 6 mm to 8 mm thick AH36 steel plates in a single pass welding using a square groove butt joint configuration. A broad range of experiments was conducted at different welding speeds and joint gaps. Initially, a suitable setting of welding speed and the joint gap was determined based on the results of penetration depth and the gap bridging ability of the welded joints. Then, the quality of the selected welded joints was examined by hardness and tensile testing. Microstructure and fractured surface analysis were carried out using scanning electron microscopy (SEM) to examine the surface morphology. Based on the experimental findings, recommendations were made for selecting suitable input welding parameters for the welding of plates up to 8 mm using the AC-GMAW process.

1. Introduction

Welding of thick steel plates is a challenging task in many industries such as shipbuilding, nuclear and power plants1,2). Different welding techniques are employed to join thick steel plates like laser beam welding, submerged arc welding (SAW) and multi-pass gas metal arc welding (GMAW)3). The laser beam welding process provide good penetration capabilities and low distortion but at the expense of high capital costs, precise fit-up requirements, extensive groove preparation and indoor welding limitations4-6). The SAW delivers high material deposition and good penetration capabilities but the amount of heat supplied to the base metal is quite high7). As a result, there is a large heat affected zone (HAZ) and a great post-weld distortion8,9). C. Shen10) reported the estimated cost of correcting the post weld distortion and it found to be as high as 30% of the total manufacturing cost. Moreover, welds produced by SAW are limited to flat and horizontal welding position11). The multi-pass GMAW process in direct current (DC) mode is employed to weld thick plates. However, high number of welding passes considerably increase the production time and cost. Compared to conventional GMAW, alternating current gas metal arc welding (AC-GMAW) is an advanced variant of GMAW process. It can be a better substitute for joining of thick plates owing to its low heat input to the workpiece and high material deposition rate capabilities12). AC-GMAW pulse works in two domains i.e. the electrode-positive (EP) and the electrode-negative (EN) domain. The arc stability is controlled by EP domain whereas high material deposition is governed by EN domain of the pulse13). D.D. Harwig14) analyzed melting rates of the process for different current waveforms. They concluded that the melting rate and the size of the metal droplet are influenced by the changing behavior of the current pulse. A.S. Nascimento et al.15) used four different waveforms with varying EN ratios to determine the suitable pulsing parameters that can provide better arc and metal transfer stability. L.O. Vilarinho et al.16) developed a methodology for the selection of AC-GMAW process parameters to reduce the arc and metal transfer instabilities. H.J. Park et al.17) analyzed the weld characteristics of dissimilar metals. They concluded that AC-GMAW process provided the good gap-bridging ability for dissimilar weld joints. A. Scotti and L.S. Monteiro18) evaluated a methodology for the input parameters selection for AC-MIG/MAG process. N. Arif and H. Chung19) measured the drop sizes using both simulation and experimental techniques for different wires of steel. D.V. Kiran et al.20) analyzed the behavior of the molten metal droplet and the welding arc at different EN ratios. K. Kim and H. Chung21) calculated the wire melting rate coefficients and developed wire melting equation based on the arc physics principles. D.D. Harwig et al.22) carried out the welding of 1.8 mm steel lap joint with a gap of 1.8 mm using AC-GMAW and pulsed GMAW. He showed that AC-GMAW provided up to 300% higher welding speeds and up to 47% less heat input as compared to pulsed GMAW process. In the beginning, AC-GMAW was applied on thin steel plates but subsequently further research work was done to extend AC-GMAW applicability for welding of thick steel plates. Regarding thick steel plate welding, the process was firstly investigated by N. Arif and H. Chung23). They observed finger-like penetration at high values of current and EN ratio. A. Ikram and H. Chung24) further researched the work and conducted an experimental study on a 5 mm thickness of steel plate. They proposed a current setting of 250 A and EN ratio of 50% for welding of steel plates where the weld joints exhibited both deep penetration and sound weld quality. However, review of the available literature has revealed that the limited findings have been reported regarding the welding of thick steel plates with the AC-GMAW process. The selection of optimum welding parameters is quite essential in welding because it determines the quality of the welded joints. Therefore, the selection of optimal welding parameters for the thicker steel plate for AC-GMAW process needs to be sought. In this paper, the work is carried out to weld 6 mm to 8 mm thick steel plates in a single pass welding. The influence of welding travel speed and joint gap on weld characteristics is investigated experimentally. Based on the experimental findings, recommendations have been made on the selection of suitable welding parameters for welding of plates up to 8 mm using AC-GMAW process.

2. Experimental procedure

2.1 Materials

High-strength low-alloy (HSLA) material AH36 was used as a base metal. AH36 is largely used in shipbuilding for ship’s hull structure. Three different thicknesses of plates i.e. 6 mm, 7 mm and 8 mm were used. The chemical composition of the base metal and filler wire (ER-70S) have been shown in Table 1 and Table 2 respectively. A steel filler wire of diameter 1.2 mm was used in the experimentation.

Chemical composition of AH-36

Chemical composition of filler wire (ER-70S)

2.2 Welding experimental set-up

Before carrying out the actual welding tests, proper alignment of two steel plates was carried out to ensure an accurate gap between joints using the magnetic clampers. The dimensions of the steel plates were 250 mm × 125 mm × 6~8 mm (thickness). A fixed gap of 1 mm or 2 mm was maintained depending upon the welding conditions. The butt-joint was made in square groove configuration and ends of plates were connected with tack welding. The welding position used in our study was flat 1G. The yield strength (YS) of the workpiece was 290 MPa whereas it had tensile strength (TS) of 485 MPa. The steel filler wire had the YS and TS of 450 MPa and 540 MPa respectively.

For conducting the welding tests, OTC-Daihen manufactured power supply DW-300 was used. The workpiece was travelled relative to the welding torch with a specific welding travel speed. A constant contact to workpiece distance (CTWD) of 25 mm was used. An average electrode extension of 18 mm was kept in all experimental runs. A mixture of shielding gases i.e. argon (Ar) and carbon dioxide (CO2) with a ratio of 80%Ar-20% CO2 was provided using a gas mixing unit. A controlled amount of flow-rate of 18 L/min was supplied. In order to visualize the molten metal droplet transfer and arc behavior, a Miro-eX4 Mono camera manufactured by Phantom was used. It recorded a video with 10,000 fps. A CAVILUX pulsed diode laser light source manufactured by High Speed Imaging Inc. was used as a back-light system to clearly visualize the mode of transfer, droplet transfer behavior and generation of spatters if present.

The welding was performed at a constant current and EN ratio of 250 A and 50% respectively. These constant parameters were selected based on the previously published literature24). However, the welding speed was varied from 4 mm/s to 16 mm/s. The joint gap of 1 mm to 2 mm was set depending on the experimental run. The experimental schematics of the process is represented in Fig. 1. It showed AC-GMAW current waveform and associated high-speed metal transfer and arc behavior. The high-speed video was synchronized with the current waveform at a different time interval to better understand the flow of metal transfer.

Fig. 1

Schematics of the welding process

3. Results and Discussion

3.1 Effect of welding speed

While maintaining a joint gap of 2 mm, welding experiments were carried out. The welding travel speed was varied from 4 mm/s to 16 mm/s with an increment of 2 mm/s. The selective results are presented in Fig. 2. Fig. 2 (a) shows the optimum welding speeds at different thicknesses of plate. The error bar represents the standard deviation. In Fig. 2 (b) the dotted line indicates HAZ and the solid line indicates fusion line. It was found that for a 6 mm thick plate, there was a good gap bridging irrespective of the welding speed and the molten metal was penetrated deep into the root at a welding travel speed ranging from 4 mm/s to 14 mm/s. This is because of the sufficient heat input supplied to the workpiece. The HAZ was found to be 52 mm2, 47 mm2 and 42 mm2 at a welding speeds of 10 mm/s, 12 mm/s and 14 mm/s respectively. It was found that the optimum welding speed was obtained in the range between 12 mm/s to 14 mm/s where the welding joints exhibited better gap bridging and complete penetration. For 7 mm thick plate, the optimum welding speed was obtained in the range between 8 mm/s to 10 mm/s where the joint exhibited the good side fusion and deep penetration with suitable bead width, reinforcement height and gap bridging. However, when welding travel speed was increased above 10 mm/s, an incomplete filling of the molten metal and lower penetration depth was observed. This is because of the fact that less heat input was supplied owing to high welding speed. The HAZ was found to be 57 mm2 and 53 mm2 at a welding speeds of 8 mm/s and 10 mm/s respectively. For 8 mm plate, welding speed in the range between 6 mm/s to 8 mm/s provided optimum material transfer rate with complete penetration depth. The HAZ was found to be 72 mm2 and 64 mm2 for a welding speed of 6 mm/s and 8 mm/s respectively.

Fig. 2

Welding joints and their penetration depths at different welding speeds

3.2 Effect of joint gaps

Based on the optimum welding speeds range determined in section 3.1, joint gap was reduced to 1 mm and welding experiments were performed. At a joint gap of 1 mm, there was a good gap bridging but less penetration depth as shown in Fig. 3. In Fig. 3 (b) the dotted line indicates the HAZ and the solid line indicates the fusion line. Fig. 3 (a) shows the penetration depth at different welding speed. It was found at a joint gap of 1 mm there was a lack of complete penetration of molten metal across the thickness irrespective of the thickness of the plate, resultant in under filing at the root side. This is because of the fact that reducing the joint gap from 2 mm to 1 mm, the molten metal could not penetrate deep into the root owing to the narrow gap between the two welded plates. The reduction in gap hindered the smooth flow of molten metal deep into the root resulted in high reinforcement height and less penetration depth. The maximum penetration was measured 3.2 mm at a welding speed of 12 mm/s, 4.3 mm at a welding speed of 8 mm/s and 5.9 mm at a welding speed of 6 mm/s for 6 mm, 7 mm and 8 mm thickness of plate respectively. Based on the research findings, it can be concluded that a joint gap of 2 mm should be maintained to fill the groove area with the molten metal otherwise reducing the joint gap may cause incomplete filling of molten metal.

Fig. 3

Penetration depth at joint gap of 1 mm with optimum welding speeds

3.3 Microstructure Analysis

The microstructure analysis of three distinctive zones including weld metal, HAZ, and base metal was performed using scanning electron microscopy (SEM) SU5000 manufactured by HITACHI, Japan. The transverse cross-section of the weld specimen was obtained through wire electrical discharge machining process. Fig. 4. shows the images obtained from the samples of 6 mm thickness, and 12 mm/s welding speed at a joint gap of 2 mm. Fig. 4 (a) is an image taken from the cross section of the welded joint which is distinctively differentiating the weld metal from HAZ, and HAZ from base metal. Fig. 4 (b) is highlighting the microstructure of the weld metal, and the fine grain size distribution is evident in the image. The fine grain size was resultant from the high cooling rate. This is because that the temperature of the weld pool was relatively high compared to the base metal close to the weld. Furthermore, Fig. 4 (c) is exhibiting an image taken from the HAZ. The HAZ is showing slightly larger grain size than from the weld metal but still finer than base metal. The decrease in grain size of HAZ has happened due to the phase transformation during the heating cycle and then cooling of the molten weld pool under ambient condition during the reverse phase transformation cycle. The microstructure of the base metal is shown in Fig. 4 (d), which is displaying significantly larger grains as compared to the HAZ, which is primarily due to prior welding larger grain size and no heat effect on the base metal during the welding. The similar trend was observed with the other thicknesses of plates at their optimum parameters condition. The different phase constituents of the welded joint were identified using optical microscopy as shown in Fig. 5. The microstructures after polishing and macro-etching (3 % Nital), the cross sections of the joints were examined. In the weld metal, the phase constituents were consisted of Widmanstätten ferrite and grain boundary ferrite. Small pits were also observed in the weld metal area. The HAZ showed fine grains. It was found that the HAZ had an average grain size of 14 µm. The decrease of the grain size was due to the high cooling rates. The microstructure of the base metal was cosnsited of the layer laminated distribution of bright ferrite and dark pearlite with grains oriented in rolling direction.

Fig. 4

(a) Cross-section of weld specimen (plate thickness: 6 mm, welding speed: 12 mm/s, joint gap: mm) (b) microstructure of weld metal, (c) microstructure of HAZ, and (d) microstructure of base metal

Fig. 5

Exhibiting various zones like base metal, HAZ and weld metal

3.4 Hardness testing

Microhardness testing has been employed and the results are displayed in Fig. 6. A Micro Vickers hardness tester (Mitutoyo, Aurora, IL, USA) was used to measure the hardness of the welded samples. The dotted line in Fig. 4 (a) shows the hardness measurement line. The hardness distribution was measured at a centerline passing between the top and bottom of the base plate. To exhibit the variation in hardness relative to the indentation area, each curve has three distinct regions where the HAZ is highlighted by the shaded region. By evaluating the data obtained from the 6 mm plates at welding speeds of 10 mm/s, 12 mm/s and 14 mm/s, it is evident that the hardness is showing an increasing trend from base metal to HAZ and fusion zone. The increase in grain size is quite understandable with the grain sizes of various regions. As the base metal has a coarse grain size, it is showing lower hardnesheetsss value i.e. 160 HV. Similarly, the decrease in grain size from base metal to HAZ, and HAZ to weld metal caused the substantial enhancement in the hardness value of the various region. Given the finer grain size in the weld metal, it is showing the highest values of the hardness i.e. 225 HV. It is clearly evident that the weld metal area at a lower speed of 10 mm/s is substantially larger than the weld metal area at a higher speed of 14 mm/s. Likewise, the HAZ is also inversely varying with the welding speed. Although the weld speeds are lower in the welding of other plates, a similar trend can be observed in both other plates with a thickness of 7 mm and 8 mm. Based on hardness data, it can be concluded that the higher the speed is better for the grain size and hardness distribution according to the distnace from the center. Moreover, the hardness of the welded specimen depends on number of parameters such as width of the weld metal and HAZ.

Fig. 6

The hardness of (a) 6 mm thick plate, welding speed: 10mm/s, 12 mm/s, 14 mm/s, (b) 7 mm thick plate, welding speed: 8 mm/s, 10 mm/s, 12 mm/s, and (c) 8 mm thick plate, welding speed: 6 mm/s, 8 mm/s, 10 mm/s

3.5 Tensile testing

Based on the selection of optimum parameters, the tensile tests were performed and the results are represented in Fig. 7. The samples were prepared according to the ASTM E8/E8M standard25). INSTRON universal testing machine 5583 with maximum 150 kN load cell capacity was used. The crosshead speed was kept at 2.8 mm/min during the test. From the findings, it can be concluded that for 6 mm steel plate, the TS i.e. 465 MPa was achieved at a welding speed of 12 mm/s which is very close to the TS i.e. 485 MPa of base metal. The TS of the welded sample was found to be 96.87 % of the base metal. However, a decrease in TS i.e. 445 MPa was measured at a welding speed of 14 mm/s with the same thickness of the plate. The percentage elongation was found to be 4.5 % and 4.1 % at a welding speed of 12 mm/s ad 14 mm/s respectively. Similarly, for 7 mm plate, a TS of 349 MPa and 337 MPa were recorded at a welding speed of 8 mm/s and 10 mm/s respectively which is 72.70 % and 70.20 % respectively of the base metal. The percentage elongation was found to be 3.1 % and 2.8 % at a welding speed of 8 mm/s ad 10 mm/s respectively. Similarly, in the case of 8 mm plate, TS of the 338 MPa was measured at a welding speed of 6 mm/s which is 70.41 % of the base metal. The percentage elongation was measured as 3.2 %. At a welding speed of 8 mm/s, TS was found to be 322 MPa which is 67.08 % of the base metal. The percentage elongation was found to be 3.1%. From the above research findings, it can be concluded that the weld joints exhibited sound weld quality. However, with the increase in thickness, the TS of the weld joints decreases. Moreover, it was found that all the welded samples were fractured at the fusion line as shown in Fig. 7 (b).

Fig. 7

(a) Tensile tests results at optimum welding parameters (b) The fractured position of the tensile tested joints

3.6 Fracture behavior

The typical morphology of the fractured surface samples obtained from tensile tests was examined by SEM. In Fig. 8 (a), fractured surface of base metal showed a complete ductile fracture having small and uniform spherical dimples since it underwent an appreciable amount of plastic deformation. This is because of the large grain size of the base metal. As slip lines are confined to the grain boundaries, the larger amount of slip can occur thus providing the greater ductility. Fig. 8 (b) shows the fractured surface for a 6 mm plate welded joint at a travel speed of 14 mm/s. The sample surface showed a ductile fracture. However, ductility of the sample was decreased compared to the base metal. This can be attributed to the relatively fine grain size of the welded joint in the fusion zone and HAZ. The finer grain size, the lesser is the ductility because the slip is restricted. Fig. 8 (c) and Fig. 8 (d) show the fractured surface for 7 mm and 8 mm and thick plate at a welding speed of 10 mm/s and 8 mm/s respectively. The fractographic examination revealed both the dimples and flat surfaces. The ductility of both the samples was decreased compared to the base metal. All the specimen underwent plastic deformation before fracture.

Fig. 8

SEM micrographs of tensile fractured surfaces

4. Conclusions

The following conclusions were drawn from the study;

  • 1) It is recommended that for welding of thick plates, the welding travel speed should be maintained in between the range of 12 mm/s to 14 mm/s for 6 mm plate, 8 mm/s to 10 mm/s for 7 mm plate and 6 mm/s to 8 mm/s for 8 mm thick steel plate. A joint gap of 2 mm should be used for welding of plates with average welding current of 250 A and 50% EN ratio.

  • 2) The microstructure of the weld metal showed the fine grain size distribution. The weld metal was consisted of Widmanstätten ferrite and grain boundary ferrite. However, the HAZ showed the slightly large grain size than from the weld metal but still finer than the base metal.

  • 3) The hardness of welded metal and HAZ was higher than the hardness of the base metal due to the local hardening phenomenon happened in the weld metal and in the HAZ.

  • 4) The welded joint exhibited good tensile properties for all thicknesses of plates.

  • 5) The fractured surface analysis of the welded specimen showed a decrease in ductility compared to the base metal. This can be attributed to the relatively fine grain size of the welded joint in the fusion zone and HAZ.

Acknowledgement

This work was supported by the research fund of Chungnam National University.

References

1. Atabaki M. M, Yazdian N, Ma J, Kovacevic R. High power laser welding of thick steel plates in a horizontal butt joint configuration. Opt. Laser Technol 832016;:1–12. http://dx.doi.org/10.1016/j.optlastec.2016.03.016.
2. Vollertsen F, Grünenwald S, Rethmeier M, Gumenyuk A, Reisgen U, Olschok S. Welding thick steel plates with fiber lasers and GMAW. Weld. World 54(3-4)2010;:R62–R70. https://doi.org/10.1007/BF03263489.
3. Ikram A, Arif N, Chung H. Design of an induction system for induction assisted alternating current gas metal arc welding. J. Mater. Process. Technol 2312016;:162–170. https://doi.org/10.1016/j.jmatprotec.2015.12.015.
4. Acherjee B. Hybrid laser arc welding:State-of-art review. Opt. Laser Technol 992018;:60–71. https://doi.org/10.1016/j.optlastec.2017.09.038.
5. Bayer E, Brenner B, Poprawe R. Hybrid laser welding techniques for enhanced welding efficiency. Proceeding of the Laser Materials Processings Conference ICALEO '96 Detroit, USA 1996;:157–166. https://doi.org/10.2351/1.5059055.
6. Ishide T, Tsubota S, Watanabe M. Latest MIG, TIG, arc-YAG laser hybrid welding systems for various welding products. Proceedings of 1st International Symposium on High-Power Laser Macroprocessing (SPIE 2003) Osaka, Japan 2002;:347–352. https://doi.org/10.1117/12.497771.
7. Aaanie J, Oguocha I.N.A, Yannacopoulos S. Effect of submerged arc welding parameters on microstructure of SA516 steel weld metal. Canadian Metall. Quart 51(1)2013;:48–57. https://doi.org/10.1179/000844311X13117643274794.
8. Joarder A, Saha S.C, Ghose A.K. Study of submerged arc weld metal and heat-affected zone microstructures of a plain carbon steel. Weld. J. Suppl. Res 70(6)1991. 141–146. https://app.aws.org/wj/supplement/WJ_1991_06_s141.pdf.
9. Lee C.S, Chandel R.S, Seow H.P. Effect of Welding Parameters on the Size of Heat Affected Zone of Submerged Welding Arc. Mater. Manuf. Processes 15(5)2000;:649–666. https://doi.org/10.1080/10426910008913011.
10. Shen C. Master of Engineering Thesis, Low distortion welding for shipbuilding industry, School of Mechanical, Materials and Mechatronic Engineering. University of Wollongong, Wollongong, Australia 2013. https://ro.uow.edu.au/theses/3892/.
11. Yadav A, Ghosh A, Kumar A. Experimental and numerical study of thermal field and weld bead characteristics in submerged arc welded plate. J. Mater. Process. Technol 2482017;:262–274. https://doi.org/10.1016/j.jmatprotec.2017.05.021.
12. Talkington J. E. Master of Science Thesis, Variable polarity gas metal arc welding, Graduate School of The Ohio State University. Columbus, Ohio, USA 1998. http://rave.ohiolink.edu/etdc/view?acc_num=osu1130352747.
13. Harada S, Ueyama T, Mita T, In-nami T, Ushio M. The state-of-the-art of AC-GMAW process in Japan. Proceedings Conference IIW, Doc. XIII-1589-1599 1999. https://ci.nii.ac.jp/naid/10030149343/.
14. Harwig D. D. Ph D dissertation, Arc behaviour and metal transfer of the VP-GMAW process, School of Industrial and Manufacturing Science. Cranfield University, Bedfordshire, United Kingdom 2003. http://dspace.lib.cranfield.ac.uk/handle/1826/11375.
15. Nascimento A. S, Fernandes D. B, Mota C. A, Vilarinho L. O. Methodology for determination of parameters for welding MIG with variable polarity. Weld. Int 232008;:473–480. https://doi.org/10.1080/09507110802543435.
16. Vilarinho L. O, Nascimento A. S, Fernandes D. B, Mota C.A.M. Methodology for parameter calculation of VP-GMAW. Weld. J 882009. 92s–98s. https://app.aws.org/wj/supplement/WJ_2009_04_s92.pdf.
17. Park H. J, Rhee S, Kang M. J, Kim D. C. Joining of steel to aluminum alloy by AC pulse MIG welding. Mater. Trans 50(9)2009;:2314–2317. https://doi.org/10.2320/matertrans.M2009105.
18. Scotto A, Monteiro L. S. A methodology for parameterization of the AC MIG/MAG process. Soldag. Insp Paulo São 17(3)2012;:271–277. http://dx.doi.org/10.1590/S0104-92242012000300011.
19. Arif N, Chung H. Alternating current-gas metal arc welding for application to thin sheets. Mater J. Process. Technol 2142014;:1828–1837. https://doi.org/10.1016/j.jmatprotec.2014.03.034.
20. Kiran D. V, Cheon J, Arif N, Chung H, Na S. J. Three- dimensional finite element modeling of pulsed AC gas metal arc welding process. Int. J. Adv. Manuf. Technol 862016;:1453–1474. https://doi.org/10.1007/s00170-015-8297-2.
21. Kim K, Chung H. Wire melting rate of alternating current gas metal arc welding. Int. J. Adv. Manuf. Technol 90(5-8)2016;:1253–1263. https://doi.org/10.1007/s00170-016-9384-8.
22. Harwig D. D, Dierksheide J. E, Yapp D, Blackman S. Arc behavior and melting rate in the VP-GMAW process. Weld. J 852006. 52–62. https://app.aws.org/wj/supplement/WJ_2006_03_s52.pdf.
23. Arif N, Chung H. Alternating current-gas metal arc welding for application for application to thick plates. Mater J . Process. Technol 2222015;:75–83. https://doi.org/10.1016/j.jmatprotec.2015.02.041.
24. Ikram A, Chung H. The effect of EN ratio and current on microstructural and mechanical properties of weld joined by AC-GMAW on square groove butt joints. Appl. Sci 7:261. 2017;https://doi.org/10.3390/app7030261.
25. ASTM E8/E8M Standard Test Methods for Tension Testing of Metallic Materials https://www.astm.org/Standards/E8.

Article information Continued

Table 1

Chemical composition of AH-36

C Si P Mn Cr S Mo Ni Cu V Fe
0.18 0.50 0.035 0.90 0.20 0.035 0.08 0.40 0.35 0.04 Balance

Table 2

Chemical composition of filler wire (ER-70S)

C Si P Mn Cr S Mo Ni Cu V Fe
0.06~0.15 0.450.75 0.025 1.401.85 0.15 0.035 0.15 0.15 0.50 0.03 Balance

Fig. 1

Schematics of the welding process

Fig. 2

Welding joints and their penetration depths at different welding speeds

Fig. 3

Penetration depth at joint gap of 1 mm with optimum welding speeds

Fig. 4

(a) Cross-section of weld specimen (plate thickness: 6 mm, welding speed: 12 mm/s, joint gap: mm) (b) microstructure of weld metal, (c) microstructure of HAZ, and (d) microstructure of base metal

Fig. 5

Exhibiting various zones like base metal, HAZ and weld metal

Fig. 6

The hardness of (a) 6 mm thick plate, welding speed: 10mm/s, 12 mm/s, 14 mm/s, (b) 7 mm thick plate, welding speed: 8 mm/s, 10 mm/s, 12 mm/s, and (c) 8 mm thick plate, welding speed: 6 mm/s, 8 mm/s, 10 mm/s

Fig. 7

(a) Tensile tests results at optimum welding parameters (b) The fractured position of the tensile tested joints

Fig. 8

SEM micrographs of tensile fractured surfaces